Skip to main content

[MW:2818] Re: 2805] Inconel 600

Hi,

 

Check www.specialmetals.com on details on Inconel 600, and www.specialmetalswelding.com  click joining brochure to know more about welding of ni-base-alloys

 

Regards,

 

Marco

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of PB HEGDE
Sent: 25 July 2009 08:30
To: materials-welding@googlegroups.com
Subject: [MW:2806] RE: 2805] Inconel 600

 

Hi!

For Inconel 600 matching consumables are

SMAW-ENiCrFe3

ii)TIG-ERNiCr3 with Nuclear grade Argon with ,Proper purging  , Use of Pulse tig ,with lower heat input will be able to produce good weld.

iii) I had experience of using Incoalloy  filler w/o any problem

iv) I have bad experience of using Mig process  hence can not share my experience

 

Other wise with good engg practices , not much problem of handling Inconel 600

 

Regards

 

Hegde

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of sorin stefan
Sent: Friday, July 24, 2009 8:06 PM
To: materials-welding@googlegroups.com
Subject: [MW:2805] Inconel 600

 


Hi Guys,
 
Please tell me what is the best match of the filer material and gas for welding ALLOY 600 ( plates 1/4"up to3/") using MIG and TIG procedures.
If you also have some welding giudelines - welding procedure regardless, it will be great
Getting an answer ASAP it will be very much apreciated
 
Thanks a lot
Sorin St.

 


Stay on top of things, check email from other accounts! Check it out.

 


lang=EN-US>


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...