Skip to main content

[MW:2754] Re: Weld Crack at Root trough weld metal

I had about the same case in my actual project, and after many tests we found that the grinding after first pass with 6010 was too deep, leaving the weld very thin, make sure to check this
 
Luis Albanés

--- El mar 21-jul-09, Antonio Ruscitto <ARUSCITT@metrogas.com.ar> escribió:

De:: Antonio Ruscitto <ARUSCITT@metrogas.com.ar>
Asunto: [MW:2748] Weld Crack at Root trough weld metal
A: "Materials & Welding" <materials-welding@googlegroups.com>
Fecha: martes 21 de julio de 2009, 10:29

Sorry IŽm forget to ask you whatŽs the thicknes of pipe?
Antonio Ruscitto

>>> "Antonio  Ruscitto" <ARUSCITT@metrogas.com.ar> 21/07/2009 11:37:31 am >>>
The WPS was qualificated? was it OK? WhatŽs kind messure value was took (Brinnel, Vickers)?
I make a WPS with first pass with E7010 and the hot pass with E8018 (Up), but maybe it better make with 100°C of preheat, and the time between first and second pass it more shorter possible after clen the fisrt pass.
Antonio Ruscitto

>>> shiva <luvshiv2002@gmail.com> 21/07/2009 10:33:36 am >>>

We are using API 5L X65 grade material for sour environment. With
reference to our WPS we used (Ador electrodes) e 8010 for root and
8018 for hot fill pass.
We took NDT and its okay. But after 1 month 4 weld joints crack. We
checked the macro hardness for existing and cracked joint . There was
a high hardness eg 351, 329 on root and in weld metal cap side 280
above. Which is very high.

Can you please tell me for this material what type of electrodes to be
used? And why this occoured ?? And what may be possible reason for
this occourance?

Regards,
Y.C.Shiva,
QA/QC Engineer,
+974 6166465
Doha Qatar.

*********************************************************************
¡IMPORTANTE!
Para evitar accidentes por inhalación de monóxido de carbono:
- Mantenga los ambientes ventilados en forma permanente.
- Revise que la llama sea color azul y uniforme.
- Instale y haga revisar periódicamente sus artefactos sólo a través de gasistas matriculados.
Recuerde que los artefactos a gas pueden emitir Monóxido de Carbono: un gas altamente tóxico e imperceptible.
Más consejos en http://www.metrogas.com.ar
*********************************************************************
Este mensaje es privado y confidencial y va dirigido sólo al destinatario indicado. Si lo ha recibido por error, por favor avísenos inmediatamente vía e-mail a error-mail@metrogas.com.ar y tenga la amabilidad de eliminarlo de su sistema. La utilización o divulgación de su contenido puede importar la comisión de un delito. No copie, reproduzca o divulgue -en forma parcial o total- su contenido. Cualquier opinión contenida, es exclusiva de su autor y no representa la opinión de MetroGAS S.A. - Muchas gracias.
This message is private and confidential and it is only intended for the addressee named above. If you have received this message and it is not addressed to you, please advise us immediately at error-mail@metrogas.com.ar and kindly remove it from your system. The use or disclosure of its contents may be regarded as an offense. Do not copy, reproduce or disclose them, either partially or fully. Opinions are the exclusive responsibility of the author and do not represent the opinion of MetroGAS S.A. - Thank you.
:: http://www.metrogas.com.ar
 



¡Obtén la mejor experiencia en la web!
Descarga gratis el nuevo Internet Explorer 8.br> http://downloads.yahoo.com/ieak8/?l=mx --~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...