Wednesday, January 19, 2011

Re: [MW:9328] QW-407.2

If your Production pwht soaking time is 10hrs, your PQR shall be qualified atleast for 80% of the 10hrs i.e. 8hrs within the same temperature range.The total time of 10 hrs can be attained in 5 cycles, each of 2 hrs or you can split it as you want by being within the temperature range.
 
However, some client specification even limit on the higher side i.e the Production PWHT soaking time shall be within 80% of the PQR soaking time. So in that case your PQR soaking time shall be within 0.8 to 1.2 times the actual production PWHT soaking time.
 
I hope it's clear.
Dokku Ajay Kumar
Mobile: +966 500071054



From: sujay kumar <sujay1199@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wed, January 19, 2011 9:56:54 AM
Subject: [MW:9322] QW-407.2

Dear Friends,
 
i need correct interperation of the Clause of mentioned below.
 
thanks and regards
 
 
 
QW-407.2
A change in the postweld heat treatment

(see QW-407.1) temperature and time range

The procedure qualification test shall be subjected to

PWHT essentially equivalent to that encountered in the

fabrication of production welds, including at least 80% of

the aggregate times at temperature(s). The PWHT total

time(s) at temperature(s) may be applied in one heating

cycle

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34916] Applicability of Impact requirement as per ASME B31.3

Dear All, Design code – ASME B31.3, Welding Code- ASME BPVC SEC IX Material  to be used used during Fabrication - SA 333Gr6 (P No.1 G...