RE: [MW:30650] Mechanical properties for SAE 1018 grade material

1018 is an AISI designation that specifies chemistry only although standards other than the general ASTM/SA-A29 might specify.  AISI 1018 is a carbon steel with a nominal carbon content of 0.18%.

 

For example:

 

A/SA-311  Specification for cold-drawn, stress-relieved carbon steel bars subject to mechanical property requirements

 

Varies on diameter/thickness

Thickness/diameter

in. (mm)

Tensile

ksi (MPa)

Yield

ksi (MPa)

Elongation - RA

< 7/8 (20)

70  (480)

60  (415)

18 - 40

>7/8 (20) to < 1¼ (30)

65  (450)

55  (380)

16 - 40

>1¼ (30) to < 2 (50)

60  (415)

50  (345)

15 - 35

>2  (50) to < 3 (75)

55 (380)

45 (310)

15 - 35

 

 

 

 

 

You might also look at other specifications referenced in A/SA-29.

 

Hope this helps.  Code is fun.  "Live long and prosper" (Mr. Spock)

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of SURESH
Sent: Monday, March 23, 2020 4:36 AM
To: Materials & Welding
Subject: [MW:30648] Mechanical properties for SAE 1018 grade material

 

Dear Expert

I am having below clarification

 

What is the mechanical properties for below said grade material, which standard to refer

1.SAE 1018

2. ASTM A29, Grade:1018

 

 

 

Regards

Suresh

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a7066f2f-0075-4d37-9c9c-f28526554fcc%40googlegroups.com.

DISCLAIMER This e-mail and any attachments thereto may contain information which is confidential and/or protected by intellectual property rights and are intended for the sole use of the recipient(s)named above. Any use of the information contained herein (including, but not limited to, total or partial reproduction, communication or distribution in any form) by persons other than the designated recipient(s) is prohibited. If you have received this e-mail in error, please notify the sender either by telephone or by e-mail and delete the material from any computer.
General Data Protection Regulation (GDPR)
We respect and protect your privacy to provide you with our services. Please read https://www.hamon.com/customer-data-protection-notice (Customer) and https://www.hamon.com/seller-data-protection-notice (Supplier) how we process your personal data.

Thank you for your cooperation.
______________________________________________________________________

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...