Re: [MW:30637] IS2062E250 WPS FOR IS2062E350

IS 2062 E250 - Tensile strength - 410 MPA & 
IS2062 E350 - Tensile strength - 490 MPA

The criterion is not only the Tensile strength, but also the metallurgical similarity, that is the reason why the P Numbers exist, but These materials do not have P Numbers assigned, see Table QW-422.
Saludos!

El jue., 19 mar. 2020 a las 8:25, Charles Jacob (<charlesvj@gmail.com>) escribió:
Dear, 

If you have qualified a base metal in a particular tensile strength, with a PNo. Then a metal with the same P No but higher tensile is not possible to weld. Your WPS cannot guarantee that weld is safe at higher tensile strengths. 


Hope this helps

Regards, 

Charles V Jacob 

On Thu, Mar 19, 2020, 4:53 PM Somnath Ashtakar <s.ashtakar@gmail.com> wrote:
Hi,

We have qualified WPS as per ASME SEC IX for material IS 2062 E250 material , now we want to weld material IS2062 E350 material, Can we use the same WPS ?

as IS 2062 E250 - Tensile strength - 410 MPA & 
IS2062 E350 - Tensile strength - 490 MPA

Please suggest your views.. Urgent.

--
Thanks and Regards,
Somnath Ashtakar

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAA484EZny6OtkXX518AU1hqCmO9J5gGU69nvMAX%3D-7v8PLfOmA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKpzM4D2yE8-vLFDTVXZozX4vACjosp9uR2cJKCxdqqT0xx-3Q%40mail.gmail.com.


--

Ing. José Juan Jiménez Alejandro

Independent Consultant in Parts

and Pressure Equipment

SSI-TPI

Móvil +52 1 812 352 4606

Skype: jjjimeneza





--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAO5ZurLABZ9UPKj6-z7trkvEi5rLLuZ5Z9wCmmfWX9H_E2m2tw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...