Skip to main content

Re: [MW:29822] HIGH HARDNESS AFTER PWHT (ER70S-2)

Yes better to change the filler wire / make and check again.

Sudheer Babu Nelapati


On Fri, Jul 12, 2019 at 6:22 AM Raghuram Bathula <raghurambathula@gmail.com> wrote:
Intersting Mr Kondori
Do you have any refernace or research paper on this subject?

Thanks

On Thu, 11 Jul 2019 at 09:23, Ramin Kondori <raminkondori@gmail.com> wrote:
Hello,

ER 70S-2 is a triple deoxidized steel welding wire. 
It has Ti, Zr, and Al additions (please check your filler metal certificate).
After PWHT, these elements can increase the hardness of weld metal (but not HAZ or base metal). Many do not consider this when choosing filler metal.
 
I recommend you to conduct a chemical analysis examination on both the filler metal (rod or electrode) and production weld metal and revert back to us. 

Regards
Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Wed, Jul 10, 2019 at 2:11 PM Karthikeyan Muthuvel <m.karthick2020@gmail.com> wrote:
Dear Experts,


Good day.


We had used the consumables (ER70S-2) / OK TIG ROD 12.62, Size : 2.4mm Dia. for our Production weld joints (Pipe materials : Carbon Steel ASTM A 106 Gr. B; Size : 3" X Sch 40). further to inform you that we had checked the Hardness of Base material , HAZ & on weld Metal before & after PWHT (below hardness readings were observed).


HARDNESS VALUES BEFORE PWHT

  1. Base material : 130 to 150 HB
  2. Heat Affected Zone : 140 to 160 HB
  3. Weld Metal : 170 to 190 HB


HARDNESS VALUES AFTER PWHT 

  1. Base material : 120 to 140 HB
  2. Heat Affected Zone : 130 to 150 HB
  3. Weld Metal : 210 to 250 HB


After performing PWHT the hardness value of Base material & Heat Affected Zone has been reduced. whereas the Hardness value of Weld Deposition has been increased (which is beyond the acceptable limit). 


So, I would like to know from you that what might be the technical reason/root cause for increase in hardness only on the weld joint after PWHT. 


Below are the PWHT parameters fyi.

Soaking Temp. : 620 Deg C

Soaking Time : 1 hr.

Rate of Heating : 100 Deg C per Hour (from 100 Deg C)

Rate of Cooling : 100 Deg C per Hour (Upto 100 Deg C)


Note:

  1. We had performed nearly 30Nos. of Production joints & we had face the problem of Hardness on all the weld joints. 
  2. Hardness was tested using Mic 10 tester method ( even cross verified with Equotip method & Tele brinell Method)


Thank you for your support.



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADxVubnMbVdbBKU-tm69PK5ZZD%2BE1kq5KW4gFtgoWp%2B6TvOYsA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOZa%2B-TwuH3TCfU5Bp-ukYHurSXcGppvVEHf-Oh%3D%2BOZ%2Bbwj%2B3Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...