Re: [MW:29839] AISI 4130 and API 5CT Well Head Casing

Dear Mr. Venkat. G

Thanks for your support and i would like to be inform if selected electrode meet NACE MR-0175 and hardness limited to 23 Max HRC
during my search i found E8018-B2 or E8018-C3 more accurate for H2S or Sure Service.

**Last question if i can use this electrode for Root or i have to select another electrode for pipe Root.      

On Wednesday, June 12, 2019 at 6:55:51 PM UTC+3, Venkat QMR (IRCA, Lead Auditor)) wrote:
Hi Ehab,
  1. E 10018-D2 - Electrode - SMAW
  2. ER 80S-D2 - FIller Wire - GTAW
You can use for SMAW first one.

Best Regards,

Venkat. G


On Wed, Jun 12, 2019 at 8:22 AM Ehab Ahmed <elpop...@gmail.com> wrote:
Dear Sirs, 

Pleas help me to Select electrode ? for AISI 4130 (70-75 Ksi) and API 5CT L80 Pipe materials to weld by SMAW. 

Using ASME IX Code.  

Thanks and Best Regards,
Ehab Ahmed

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20385728-b6dc-46fa-b65c-7fc06c8a7b47%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
Venkatachalam Govindan
QHSE Lead / Trainer
(IRCA Registered Lead Auditor & API / CQI Practitioner)
+965 97604989, +919840502376 (
WhatsApp only)

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e1394032-53d1-4d9d-976c-880537c6f1a0%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...