Skip to main content

Re: [MW:29788] SA420 Gr. WPL6/SA234 Gr. WPB

Dear dual product may possible if follow & meeting criteria. 

Please review MTC. 

Regards

Dinesh

On Saturday, July 6, 2019, 'anand gupta' via Materials & Welding <materials-welding@googlegroups.com> wrote:
I think it was punch by mistake. 
No body manufacturer one product with dual spec. 

Regards 
A p gupta 
ThyssenKrupp 
Qc manager 


On Sat, 6 Jul 2019 at 9:20, U2L Poenya

Thank's for your advice sir..

But, why the manufacture make the product with double spec in same of part

 

Thanks

 

 

SuLfi

 

Sent from Mail for Windows 10

 

From: anand gupta
Sent: Saturday, 6 July 2019 10:12 AM
To: materials-welding@googlegroups.com; Sulfi Afdhal; Materials & Welding
Subject: Re: [MW:29780] SA420 Gr. WPL6/SA234 Gr. WPB

 

WPB is for high temp and WPL6  is for low temp. 

You can not use. 

 

Regards 

 

A p gupta 

ThyssenKrupp 

Qc manager 

 

On Fri, 5 Jul 2019 at 19:36, Sulfi Afdhal

Dear

 

I have a question about my Inspection Certificate of pipe fitting.

We order of material for low temperature ASTM A420 Gr. WPL6.

But, in hard stamp and certificate is "WPL6/WPB" (Attached)

Where i know, for WPB is ASTM A234.

what is the product can used for Low Temperature Service -45degree Celcius???

and if true, any one know reference from standard ASTM???

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4d83d7bf-10a1-4d0e-8cb7-6a0efd0c7679%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/126229978.3677541.1562400848720%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.


--
Thanks & Regards

DINESH VITTHAL SOMWANSHI

BACHELOR IN MECHANICAL ENGINEER

AUTHORIZED PIPING / WELDING / NDT / PAINTING INSPECTION PERSONNEL
API 570 - Piping Inspector, AWS - CWI , CSWIP 3.1*,*BGAS  Gr 2 / 3
NDT II -UT , RT , MT , PT, VT
 00919881344135 India 
Skype = dinesh somwanshi

असो द्यावी दया तुमच्या लागतसे पाया.

*Pray for others, sometime, You might never need to pray for yourself
again.....*


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAELgRrXqC5__LV39dAmObsq1O4cBSoU3XUyBbXQUB9JPzwxPaQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...