Skip to main content

Re: Re: [MW:28459] WELDING P11 WITH P91 STEEL

Welding with pup piece you get one similar and one dissimilar obviously you will have two Weld joints, in this case you have to have two pqrs or you have to prepare a dissimilar pqr incorporating similar, possible? with pwht values within the tolerances? Filler etc? 

Welding without pup piece Piping we have did same scenario with dissimilar pqr for power generation high steam boilers. 

On Sat, Oct 20, 2018, 4:01 PM Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
When u weld P11 directly with P91 and then SR at 760°C will be very close to Lower critical temperature of P11 material. So better to have pup piece in between them. 

On Fri, 19 Oct 2018 9:21 pm muneebslsa@gmail.com, <muneebslsa@gmail.com> wrote:

Firstly, I do not understand the consequences of all 3 for what is the purpose?

Secondly, ok if you are doing butter there may be some purpose but scenario 1 and 3 why?

I feel like scenario 3 pub piece for tie in? Or shut down? If this is the case I agree with scenario 3.

Or

Scenario 1.

Still the questionnaire has deep knowledge of scenario than the one who is giving answer, to be precise, need more clarity for more information.


Regards,

 

Muneeb.M





 
Date: 2018-10-19 16:03
Subject: Re: [MW:28445] WELDING P11 WITH P91 STEEL
Weld p22 and P91 (Pup piece) and SR. Then join p11 with p22. 

On Fri, 19 Oct 2018 4:27 pm DDN VERMA, <vermananhu@gmail.com> wrote:
Dear Sirs,

I read several methods to join a P11 [1.25 Cr- 1/2 Mo] pipe to P91 [9Cr - 1 Mo] pipe, such as :

1. Weld using filler metal corresponding to corresponding to [2-1/4Cr - 1Mo] steel & post weld heat treat at appropriate temp..

2. Butter P91 with  filler corresponding to  [2-1/4Cr - 1Mo], post weld heat treat & weld with P11 & re-post weld heat treat it.

3. Use a P22 pup piece to join P11 with P91, etc. etc.....  

However, I wish to know, which is the most appropriate method taking into considerations the overall weld-integrity and high temperature strength of the weldment.

Please help to clarify my doubts.

THANKS,
DDN VERMA

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...