Re: [MW:27521] Nick break test

1. It looks like the row of interlocked pores near one external surface of the fracture-surface could be giving you more of a notch-effect (aka "stress-concentration") than in a defect-free sample.
2. A possible cause of the pores are poor shielding of the arc due to moisture-entrainment.
3. The nick-break test was developed at Lehigh University in the the middle of the last century. Why are you using it now? An example of the use of this test is in the Welding Journal in about 1955, by W.J.Murphy and Robert Stout.

Ed Dalder
Very old welding metallurgist.

On March 15, 2018 at 2:59 AM Mani kandan r <manikandanr21@gmail.com> wrote:

Dear gents,

Pls find the attached Nick break test coupon, what is the type of defect? & how to control this?

Process -GTAW+ SMAW

Thanks & Regards,

R.Manikandan

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...