Skip to main content

RE: [MW:25300] Pitting corrosion test failure

Dear All,

Thank you all fr your great inputs..lot of learning!!

We have re tested according to shell dep fr welding of dss  with another cut piece grom the same pipe with flat specimen(2nos) and ensured proper finishing and avoided sharp edges, proper passivation n pickling. We could get the value of 1.3g/sq.m which was accepted by customer.

Regards
Prasad


On 22 Aug 2016 6:54 a.m., "pgoswami" <pgoswami@quickclic.net> wrote:
Mr. Prasad,
 
You've problem with shielding gas selection. For Any DSS or SDSS, Ar+N2(up to 2%) is considered to be beneficial to balance the Ferrite+Austenite Ratio.It's the proven truth.
Typically DSS 2205 should pass the ASTM G-48A test if welded with due care, shielding gas selection etc.
 
Surface preparation etc  may help, however competent Lab personnel would very well know what to do about surface preparation.
 
In the same note did the BM and Filler metal were tested for G48A test.That's important.
 
Hope the above tips would help you.
 
Look forward to your response.
 
Thanks.
 
 

 

Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineering Specialist ,

Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 



From: 'Mohammed Rafiuddin' via Materials & Welding [mailto:materials-welding@googlegroups.com]
Sent: Sunday, August 21, 2016 3:33 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:25273] Pitting corrosion test failure

Mr.Prasad,

ASTM G48 test is considered to be a check of metallurgical condition of DSS rather than of its performance in any service environment.

We had a similar case.Then client requirements changed and it was asked to perform test according to ASTM A923 Method C which we passed.

Consult your client this may help you.

Regards,
Mohammed 


On Saturday, 13 August 2016 6:25 AM, "nithindsilva4u@gmail.com" <nithindsilva4u@gmail.com> wrote:


Hi,
At the below temperature it should pass. Is your end product will be picked and passivated?? If yes, pls do the picking and passivation of test sample, it should pass.

Sent from my iPhone

On Aug 12, 2016, at 09:50, Harish Kannepalli <harishkannepalli@gmail.com> wrote:

Hi Prasad,
Most of the tests fail also due to improper sample preparation or wrong dimensions during calculation of weight loss. Ask for a retest for 2 samples.
Regards
Harish.

On Aug 11, 2016 10:31, "Prasu Cutie" <pracuty@gmail.com> wrote:
Dear experts,
We had pittng corrosion failure in duplex stainless  steel 2205
Process: GTAW
Thk: 7.62mm
Filler: ER2209
Product: pipe
Heat input observed: 1.5 to 2.5kj
Gas: argon 99.9997purity
Weight loss reqd is <4g/sq.mtr, achieved 21g/sq.mtr
Testing is done as per ASTM G48
Can any one tell me why this failure occured, what could be the reason?
Regards
Prasad
--
http://www.linkedin.com/ groups/MaterialsWelding- 122787?home=&gid=122787&trk= anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
To post to this group, send email to materials-welding@ googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ CAKgcArS8ogq8UVK8TnByOg9L7Garx aej2a1pwHyQ8iR9MeSRuQ%40mail. gmail.com.
For more options, visit https://groups.google.com/d/ optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAE4SttF3c7oZ3s8yst9h_FAbwsfYwCfYtdGJkDmmXRkKBBmaeA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/17749109-FB1C-4A64-99B4-50A6959BEA47%40gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/940908731.15520896.1471764766626.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/D68E4A29CFEE406ABD5915F71BCA3897%40homepg.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKgcArQjvBvf5sCmBuzZRB0KGhxRR48u4wovOe%2BA8j_%2BB36h9Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...