actually I need to mention an flange thickness instead of flange width(machining partially are not allowed on rf)


On Sat, Aug 3, 2013 at 2:36 PM, Dinesh Somwanshi <som.din@gmail.com> wrote:

 dear Krishna,
 
as per my kwoledge & information,generally we are following for serration damage is as,
 
1.serration inspection is based on comparative method for the serration (using comparator)
 
2.if possible the width of the flange as per 16.5 permit some tolerance if its extra you make machining for raised face (mim 1.6 -2 mm)with respect to flange face.
 
if its width of flange is outside tolerance limit ,to avoid delay better for replace new one.but this also based on clint contractor mutual understanding & terms..
 
regards
 
Dinesh somwanshi

 
On Fri, Aug 2, 2013 at 11:11 AM, Badam krishna <krishna.1828bv@gmail.com> wrote:
Dear Experts,

1.Share your Knowledge on Serration damage on flange face
2. B 16.5 allows serration damage allowance/acceptance criteria (Table 3) . explain how to interpretate?
3.Welding can be permitted for flange face/Serration damage? 


with regards,

B.KRISHNA

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...