Re: [MW:14695] Dissimilar Welding: 5Cr-0.5Mo Furnace Tube with SS304 Guide pin

Dear Mohammad Ali

As per AWS D10.8(RP for Welding of Cr-Mo Steel Piping & Tubing) you can use ENiCrFe-2 or -3 for SMAW process and ERNiCr-3 for GTAW and GMAW process, meanwhile for non-cyclic thermal service up to 600° F (315°C) type E309 or E309Mo stainless steels filer metals frequently used.

Regards,
Himan Nikdin

On Tue, Jun 26, 2012 at 12:47 PM, ESMAT S <ss824@hotmail.com> wrote:
I face this problem but with ss316 to p91 (9cr) in steam line and the welding was buttering procedure with the higher grade which is p91(9cr) filler.
Generally the dismiler Welding should be with the higher grade material according to the code . 

Sent from my iPhone

On Jun 26, 2012, at 11:06 AM, "M. Ali Halai" <mali5286@gmail.com> wrote:

Dear All,
 
We have to weld an Ø1½" SS 304 guide pin pipe to Ø4" 5Cr furnace tube. I was unable to find any WPS in our records. Some research I did revealed that I should be using SS 309 for the welding. What I am concerned is whether Stress relieving is necessary? I learned from somewhere that it will lead to sigma phase creation and carbide percipatation in austenitic stainless steel.
 
Your comments / help is much appreciated.
 
 
Regards,
 
Muhammad Ali

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...