Re: [MW:14645] Re: welding procedure qualification requirement for P No.1 Group no 1,2

Hi,
 
In that case, qualify SA 516 Gr. 60 + 70 in a Single Test Coupon, so that U can have 3 WPSs, P No.1 Gr 1 TO 1, Gr. 1 to 2, Gr. 2 to 2 for Impact tests and U need to test in both Gr.60 HAZ & Gr.70 HAZ additionally, refer spec and codes requirements for Impact testing.
 
 
Refer the below statement from ASME-IX,
 
 
QW-403.5 ( C ) In addition, when base metals of two different
P-Number Group Number combinations are qualified using
a single test coupon, that coupon qualifies the welding of
those two P-Number Group Numbers to themselves as well
as to each other using the variables qualified.
 
 
Regards,
Sarav,
Korea

On Fri, Jun 22, 2012 at 12:44 AM, Raghuram Bathula <raghurambathula@gmail.com> wrote:
sorry, typo error, yes it is QW 403.5

On Jun 21, 2:06 pm, "Jambhale, Rupesh A" <Rupesh.Jambh...@mottmac-
india.com> wrote:
> I think its a  QW 403.5
>
>
>
>
>
>
>
> -----Original Message-----
> From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Raghuram Bathula
> Sent: 21 June 2012 14:26
> To: Materials & Welding
> Subject: [MW:14633] Re: welding procedure qualification requirement for P No.1 Group no 1,2
>
> yes, refer QW403.6
>
> On Jun 21, 1:47 pm, LALIT VADADORIYA <lalit.vadador...@gmail.com>
> wrote:
> > Dear expert,
>
> > If welding procedure is qualified for the SA 516 Gr.60 to same (P No.1
> > Group 1 to same), then is it required to conduct another PQR for the
> > SA 516 Gr.70 to same (P No.1 Group 2 to same), if impact requirement
> > is applicable for both material at same temperature?
>
> > --
> > Regards
>
> > *Lalit Vadadoriya
> > Sr.Engineer (Inspection)
> > Engineers India Limited*
> > *Dahej Petrochemical Complex,*
> > *Dahej (Gujarat)*
> _______

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...