Thursday, June 21, 2012

RE: [MW:14635] RE: 14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.

You are correct.  Per QW-200.4(b), the fill process PQR/WPS must be thicker than that for the root process.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of yash yagnik
Sent: Thursday, June 21, 2012 1:23 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:14630] RE: 14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.

 

Dear Mr John,

Your reply is absolutely spot on and only thing required to add into this is :

For QW 200.4 (b) in regards the example explained by you for GTAW and SAW process : GTAW PQR with 13mm thickness combined with a SAW PQR - it is mandatory requirement that SAW process PQR shall have greater thickness than GTAW PQR base metal , hence it shall be greater than 13mm.

I hope this is correct and inline with ASME SECTION IX.

Please share your views if any.

Regards

Yash Yagnik

On Wed, Jun 20, 2012 at 1:47 AM, John Henning <jhenning@deltak.com> wrote:

Mr. Mohammed-Al-Wi,

Respectfully, you response is incorrect for the situation described.  I believe Mr. Nakwal is asking if he can take a PQR performed with two process and split them into two separate WPS's, one for each process.  This can be done per the last paragraph of QW-200.4(a) which states;
"When following a WPS that has more than one welding process, filler metal or set of variables, each process filler metal, or set of variables may be used individually or in different combinations provided  (1) the essential, non-essential, and required supplementary essential variables associated with the process, filler metal, or set of variables are applied   (2) the base metal and deposited weld metal thickness limits of QW-451 for each process , filler metal, or set of variables are applied.

So, Mr. Nakwal has a PQR performed on base metal 8mm thick, with 3mm GTAW deposited metal and 5mm SMAW deposited metal.

Per QW451.1, it qualifies for GTAW:  Base metal thickness 1.5mm ~ 16mm, and deposited GTAW filler metal to a maximum of 6mm
And it qualifies for SMAW:  Base metal thickness 1.5mm ~ 16mm, and deposited SMAW filler metal to a maximum of 10mm

I suggest looking at Interpretations IX-78-47, IX-86-23 Q1 & Q2, IX-95-10, and IX-04-08.  In addition, you might want to look at Interpretations IX-81-32, IX-86-01 and IX92-97.

QW-200.4(b) applies only when trying to COMBINE two PQR's with into a single PQR, where a minimum of 13mm must be welded with the root process in order to "ride along" with the fill process to the maximum that fill process is qualified for.  An example would be a GTAW PQR with 13mm thickness combined with a SAW PQR with 38mm thickness to yield a WPS with a GTAW root and SAW fill qualified to for base metal thickness range of 5mm to 200mm.  The GTAW process in this example would be limited to a deposited thickness of 26mm.

Let me know if you have any questions.

John A. Henning
Welding & Materials

-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of ahmraha@yahoo.com
Sent: Tuesday, June 19, 2012 8:39 AM
To: materials-welding@googlegroups.com
Subject: [MW:14600] RE: USE of PQR of GTAW+SMAW for new WPS GTAW process only.


-----Original Message-----
From: mohd
Sent:  15/06/2012, 9:53  am
To: Materials & Welding
Subject: [MW:14556] Re: USE of PQR of GTAW+SMAW for new WPS GTAW process only.


Dear all,

if you go through 200.4(b) For GTAW, SMAW, GMAW, PAW, and SAW, or combinations of these processes, a PQR for a process recording a test coupon that was at least 1⁄2 in. (13 mm) is required hence u cant creat two WPS.

Regrds,
Mohammed-AI-WI.



On Jun 11, 5:02 am, Parveen Kumar Nakwal <pknak...@gmail.com> wrote:
> Dear Experts,
>
> Can we use S.S to S.S 8mm base metal thickness PQR of GTAW (3mm)+SMAW
> (5mm) for the making for new WPS of S.S to S.S with GTAW only, with
> 2mm base metal thickness only ?
>
> Waiting for reply..
>
> Regards.
> Parveen K. Nakwal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

No comments:

Re: [MW:35737] Bend Test and Tensile Test failed for ET45 Micro Welded Coupon

Hi As its %elongation is very low  Better try buttering on jt surrace with ductile consumable like pure Ni i. E Ni1 And later weld jt with c...