Hi Nilesh,
'matter of fact the lower range value is equally important. If the heat input is reduced as compared to PQR values, tendency to harden increases as cooling rate is increased. In your WPS, you need to mention the range as recorded in the PQR.
TG--On Fri, Mar 23, 2012 at 11:53 AM, Prashant Shelar <pshelar@lamprell.com> wrote:
Hi Nilesh,
Being impact as a requirement, you will have to limit the maximum Heat Input value in WPS as qualified in the PQR. You will have to indicate the values on WPS with upper limit restricted to that in PQR.
Thanking you,
Rgds,
Prashant
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of waman nilesh
Sent: Friday, March 23, 2012 11:07 AM
To: materials-welding@googlegroups.com; materials-welding@goolegroups.com
Cc: wamannp@yahoo.com
Subject: [MW:13977] Heat input value in WPS
Dear Experts,
I have question we are doing WPS, PQR & WPQ ( Material- IS 2062 GR B & thickness- 20 mm ) as per EN 15614 standard in which impact is essential.
So which value of heat input is to be mention on WPS.
With Regards,
Nilesh
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Any views or opinions expressed in this email and its attachments are those of the individual sender except where the sender specifically states them to be that of Lamprell.
This E-mail and any attachments are confidential and may also be legally privileged. If you have received this email and any attachments in error, you are on notice of its status. Please (a) notify the sender immediately by reply email; (b) destroy this email and any attachment, and (c) do not use, copy, store and/or disclose to any person this email and any attachments: to do so could be a breach of confidence. Thank you for your co operation. Please contact the Lamprell IT Helpdesk on ithelpdesk@lamprell.com if you need any assistance.
Holding company: Lamprell plc, incorporated in the Isle of Man, registration number 117101C, registered office at Fort Anne, Douglas, Isle of Man IM1 5PD
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Tarantula
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments