Re: [MW:8613] INCONEL 625 OVELAY ON SA 516 GR 70

Hi!
Generaly for Inconel 625 Fe is restricted to max 5% and if you want to reduce the Fe% we require to
i) Ask Electrode manyfacturer to get the elctrode with lesser Iron % which is being suppled by reputed mfgr like Spl metal,Bohler, or even L&T  EWAC
as per our requirement
ii)Some time it is advisible to use 3 layers of overlay for SMAW or GTAW process
iii) You can achieve less than 5% say up to 3% by ESSC process
 
For such stringent requirement you need to establish the parameters and overlay technique
 
Regards
 
Hegde p.B.

 


From: PREM SHANKARDUTT NAUTIYAL <prem_nautiyal@rediffmail.com>
To: materials-welding@googlegroups.com
Sent: Wed, 8 December, 2010 9:21:42 PM
Subject: Re: [MW:8601] INCONEL 625 OVELAY ON SA 516 GR 70

Hi

Are you talking about max. Fe (iron) content ?
Ferrite content in overlay of Inconel 625 deposit ???
How much is the required overlay thickness ?
Please clarify...

Regards

Prem Nautiyal


On Wed, 08 Dec 2010 12:30:02 +0530 wrote
>Dear All,





I've got a doubt on the following issue,



We're going to make an overlay with INCONEL 625 over SA 516 Gr. 70

(60mm thick) on its edge. But when we do the PQR for this the ferrite

content on this overlay is found to be 4%. Is there any standard

restricting this??? Because my client is asking for a max. of Ferrite

content of 3%.







Please Reply.







Regards



Akhil



--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



PREM S NAUTIYAL
CELL : 9769316004

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.