[MW:8527] Re: cracks in tacking

vasu,

we are also have the same problem before, i am suggesting you to put a
tacking bridge same material as base metal and to be tack in bevel
face and increase the preaheat temp. up to 177-180 deg. celcius

marcelo p. soriano
qa/qc eng'r

On Dec 3, 7:37 am, srinivas rao <ksrv...@gmail.com> wrote:
> Dear All,
>
> we are using  FILLER WIRE ER 90SB3 FOR SA387GR22 CL-2 thk 6mm...we are are
> pre-heating to 150 with  torch....after doing tacking, about 95% of tacks
> are found to have cracks .We have not released for Welding.The filler
> material is checked and ok. pls give your sugestions.
>
> Regards
>
> Vasu

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...