Re: [MW:8427] HOTTAP on SOUR LINE (PWHT Required)

If thickness is coming out more than code requirement, you may have to do PWHT. For on line service welding, PWHT is not practically possible at site. You may have to choose compatible material, FEA analysis, ECA analysis..


Thanks,
H Solanki

On Mon, 29 Nov 2010 09:03:56 +0530 "Majdi N Elyyan" wrote
>

Dear All;

We have a hot tap on LPG line (Sour service) which require PWHT.

The run Pipe is 4", the branch is also 4", split tee will be used.

As per shell DEP-31.38.60.10 – for Hot tapping, clearly mention:

Hot-tap welding should not normally be performed on materials which require post-weld

heat treatment. However, if stress relieving or post-weld heat treatment is required, a

specialist shall be consulted to assess whether it is feasible to make the specific

hot-tapping operation with post-weld heat treatment.

Note: Stress-relieving may be required if a material is susceptible to stress corrosion cracking and post-weld

heat treatment may be specified by the design code if the wall thickness is greater than a certain limit.

& since we have no other options, we have to do the hot tap on the same, kindly advice WPS & PWHT procedures

Thank all in advance..

Regards

Majdi Elyyan

--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .