Skip to main content

RE: [MW:8358] RE: 8318] Tandem SAW - optimum thickness

I have used tandem SAW for as thin as 9mm square butt welds for
longitudinal and girth welds on shells, 100% penetration and 100% UT
inspection. (Single pass inside & outside.)

A few notes:
1. A good fit-up is required, any gaps and one will blow-through.
2. Watch the ID as you place the outside pass. a Medium orange color if it
starts getting too bright reduce the current quickly, or you end up with a
burn-through.
3. Watch the spacing between the electrode, too little the arcs interfere
with each other too large and the out-gassing of the leading arc will cause
problems with the trailing arc.
4. Thinner shells were run on a head & tail stock machine with a C&B. Heavy
shells on a roller bed with a C&B.
5.If one has a poor fit-ups use GMAW to add a filler to close.


Richard Beldyk CWEng

Original Message:
-----------------
From: Garry Hunt garryhunt8@msn.com
Date: Tue, 23 Nov 2010 12:18:14 +0000
To: materials-welding@googlegroups.com
Subject: RE: [MW:8355] RE: 8318] Tandem SAW - optimum thickness

Good morning

Why not use strip?


Date: Mon, 22 Nov 2010 17:03:55 +0000
To: materials-welding@googlegroups.com
Subject: Re: [MW:8351] RE: 8318] Tandem SAW - optimum thickness
From: prem_nautiyal@rediffmail.com

Hello Shadab


I was plaanning to use Tandem SAW for 25mm thk butt joint in a shell of @3m
dia.

I had gone through various literatures of reputed consumable manufacturers
wherin it was mentioned that tandem SAW can be used for 15mm thickness and
above. But if you see practically tandem SAW will cause distortion and
ovality in thin walled shells in shop!!

Thus i am very much convinced by what Mr.Hegde has practically recommended
i.e 35mm thickness and above..

Regards

Prem Nautiyal
Thermax Ltd, Pune, India.


On Sat, 20 Nov 2010 09:05:38 +0530 wrote
>

Dear Prem,

You can use Tandem
welding from 6mm and above as per Lincoln's recommendation.

Still in Godrej?

Thanking you,

Best regards,

Shadab Alam Ansari

Welding Engineer

From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of PREM
SHANKARDUTT NAUTIYAL

Sent: Friday, November 19, 2010 6:54 AM

To: materials-welding@googlegroups.com

Subject: [MW:8318] Tandem SAW - optimum
thickness

Hi friends

I would like to know the "Optimum thickness" of shell wherein we can
use Tandem SAW.

The shell MOC is SA516Gr.70.

Regards

Prem Nautiyal

PREM S NAUTIYAL

CELL : 9769316004

--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at
http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t.
applicable code/standard/contract documents.

--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.
>


PREM S NAUTIYAL
CELL : 9769316004

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.


--------------------------------------------------------------------
mail2web.com – What can On Demand Business Solutions do for you?
http://link.mail2web.com/Business/SharePoint


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...