Re: [MW:8357] 8318] Tandem SAW - optimum thickness

It is a groove weld in a 25mm thk shell with double V butt joint.

PREM S NAUTIYAL
CELL : 9769316004

On Tue, 23 Nov 2010 23:06:30 +0530 "Potter, Richard" wrote
>

Is this an overlay operation or a grooveweld????


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Garry Hunt
>Sent: Tuesday, November 23, 20106:18 AM
>To: materials-welding@googlegroups.com
>Subject: RE: [MW:8355] RE: 8318]Tandem SAW - optimum thickness

Good morning
>
>Why not use strip?
>


Date: Mon, 22 Nov 2010 17:03:55 +0000
>To: materials-welding@googlegroups.com
>Subject: Re: [MW:8351] RE: 8318] Tandem SAW - optimum thickness
>From: prem_nautiyal@rediffmail.com
>
>Hello Shadab
>
>
>I was plaanning to use Tandem SAW for 25mm thk butt joint in a shell of @3mdia.
>
>I had gone through various literatures of reputed consumable manufacturerswherin it was mentioned that tandem SAW can be used for 15mm thickness andabove. But if you see practically tandem SAW will cause distortion and ovalityin thin walled shells in shop!!
>
>Thus i am very much convinced by what Mr.Hegde has practically recommended i.e35mm thickness and above..
>
>Regards
>
>Prem Nautiyal
>Thermax Ltd, Pune, India.
>
>
>On Sat, 20 Nov 2010 09:05:38 +0530 wrote
>>
>
>
>
>Dear Prem,
>
>You can use Tandem
>welding from 6mm and above as per Lincoln'srecommendation.
>
>Still in Godrej?
>
>
>
>Thanking you,
>
>Best regards,
>
>
>
>Shadab Alam Ansari
>
>Welding Engineer
>
>
>
>
>
>From: materials-welding@googlegroups.com
>[mailto:materials-welding@googlegroups.com]On Behalf Of PREM
>SHANKARDUTT NAUTIYAL
>
>Sent: Friday, November 19, 2010 6:54 AM
>
>To: materials-welding@googlegroups.com
>
>Subject: [MW:8318] Tandem SAW - optimum
>thickness
>
>
>
>
>
>Hi friends
>
>
>
>I would like to know the "Optimum thickness" of shell wherein we can
>use Tandem SAW.
>
>The shell MOC is SA516Gr.70.
>
>
>
>Regards
>
>
>
>Prem Nautiyal
>
>
>
>PREM S NAUTIYAL
>
>CELL : 9769316004
>
>
>
>
>
>
>
>
>
>--
>
>To post to this group, send email to materials-welding@googlegroups.com
>
>To unsubscribe from this group, send email to
>materials-welding+unsubscribe@googlegroups.com
>
>For more options, visit this group's bolg athttp://materials-welding.blogspot.com/
>
>The views expressed/exchnaged in this group are members personel views and
>meant for educational purposes only, Users must take their own decisions w.r.t.
>applicable code/standard/contract documents.
>
>
>
>
>
>
>
>
>
>--
>>
>To post to this group, send email to materials-welding@googlegroups.com
>>
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>>
>For more options, visit this group's bolg athttp://materials-welding.blogspot.com/
>>
>The views expressed/exchnaged in this group are members personel views andmeant for educational purposes only, Users must take their own decisions w.r.t.applicable code/standard/contract documents.
>>
>
>
>PREM S NAUTIYAL
>CELL : 9769316004


>--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email tomaterials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views andmeant for educational purposes only, Users must take their own decisions w.r.t.applicable code/standard/contract documents.

--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...