Skip to main content

[MW:3815] RE: 3807] Welding of P5A & P5B Material

See below -

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of KC
Sent: Wednesday, December 09, 2009 1:44 AM
To: Materials & Welding
Subject: [MW:3807] Welding of P5A & P5B Material

Can any body inform about the .....

For the welding of SA 335 Gr. P91 (PNo-5B, Group No-2) Material.........
1) What is the Preheating Temperature? 400F (200C)
minimum
2) What is the Post heating Temperature & Time ? Typical 1400F
+/- 25F (760C +/- 15C)
3) PWHT is require or not ? P91 should
always be PWHT'ed, only exception - ERW tube finning with qualifiers
4) While welding (GTAW) Backing is require if yes, then Argon is OK
? P91 open root welds should always be gas backed with Argon due to
high Cr.

For the welding of SA 335 Gr. P22 (PNo-5A, Group No-1) Material.........
1) What is the Preheating Temperature? 300F (150C)Code
minimum, I recommend 400F (200C)
2) What is the Post heating Temperature & Time ? Depends on
Code: Sec I or VIII 1250F (675C) min.; B31.X 1300F (705C) min.
3) PWHT is require or not ? Depends on (1)
Code and then (2) thickness, (3) diameter, and (4) type of weld -
insufficient detail
4) While welding (GTAW) Backing is require if yes, then Argon is OK
? Not required by Code, some customers want it others do not. My
opinion is that Cr content low enough it is not really required except
perhaps for highly aggressive corrosive environments certainly should
not be necessary for steam service.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...