Skip to main content

[MW:3562] RE: 3559] CONSUMABLES

First idea is to use CrMo2 consumables (or CrMo1 could be solution too, depending on application / requirements)

Preheat 200 degrC

PWHT at 690 °C , however

·         PWHT temperature is depending on strength requirements 4130 and required charpy values in weld metal

·         duration is depending on wall thickness and required charpy values in weld metal

 

Stick electrodes

·         OERLIKON CROMOCORD 2 STC

·         OERLIKON OE KV3 HR

TIG rod:

·         OERLKON CARBOROD CrMo2  or

·         OERLIKON CARBOROD KV3 (=B2)

 

Erwin Gering

AIR LIQUIDE WELDING

OERLIKON_RVB_5cm.BMP

 

Van: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] Namens rajagopal kannan
Verzonden: woensdag 28 oktober 2009 8:23
Aan: materials-welding@googlegroups.com
Onderwerp: [MW:3559] CONSUMABLES

 

Dear Members,

Could you please suggest me the apt consumable for GTAW and SMAW to weld SA 182 Gr. F22 cl.1 with AISI 4130?

Thanks and Best Regards,

K.Rajagopal



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...