Skip to main content

[MW:3391] Re: 3297] 3295] Welding qualification of very low sulfur steels.

I'm a member of this group and have been following this discussion with some interest. I am attaching a summary of a position on the need for controlling the S level in type 316LN stainless steel that will be autgeneously G.T.A welded in the form of small diameter thin-walled tube. Any comments or feedback is welcomed. I also hope that some of the information that I'm posting will be of value to others.

Ed Dalder


----- Original Message -----
From: "John Henning" <jhenning@deltak.com>
To: materials-welding@googlegroups.com
Sent: Tuesday, September 29, 2009 7:43:31 AM GMT -08:00 US/Canada Pacific
Subject: [MW:3371] RE: 3297] 3295] Welding qualification of very low sulfur steels.

In the past, super clean steels were investigated by EPRI and others.  It was found that if the sulfur is extremely low, one can experience arc wander and significant difficulty in obtaining a quality weld.  Just a wee bit is good thing from a welding stand point.  I don't have access any longer to these reports so I cannot provide any additional information.
 
John 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram (Mumbai - PIPING)
Sent: Wednesday, September 23, 2009 11:53 PM
To: materials-welding@googlegroups.com
Cc: piping_valves@yahoogroups.com
Subject: [MW:3297] 3295] Welding qualification of very low sulfur steels.

Dear Kannan

Welcome on board after long time

 

Before seeing the link provided below, I thought you were asking for a CS material, and quite surprised by this claim that low sulfur will affect the weld quality?

Sulfur is an impurity in terms of steel making, and even weldability point of view, it was never an issue at least for process plant equipment or piping welding, the lower is the better.

It is quite common for offshore O&G application (where HIC/SOHIC/SSCC is envisaged) with such low sulfur content (Dillinger is one such manufactures for plates, their Dicrest series plates are guaranteed with S £ 0.0010 %).

Your specified sulfur conentnt restriction is for SS or CS ( or Duplex?)

 

The article mentioned in the below link related to small dia SS tubing welded with Autogenous Orbital GTAW, it's a typical case. Never an issue for our type of applications  


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of S. Kannan
Sent: Thursday, September 24, 2009 12:05 AM
To: materials-welding@googlegroups.com
Subject: [MW:3295] Welding qualification of very low sulfur steels.

 

----- Forwarded Message ----
From: kannan_cit <kannan_cit@yahoo.com>
To: piping_valves@yahoogroups.com
Sent: Wednesday, September 23, 2009 7:26:46 PM
Subject: [piping_valves] Welding qualification of very low sulfur steels.

 

Quit some time ago, I was having great difficulty in finding mills manufacturing steels with sulfur limited to 0.001% max. due to a wrong prescription by one of the well known PMC. Though it was resolved with higher relaxation later, I started to look into the issues concerning the restrictions posed in the sulfur content in steels, which were mainly added to increase the machinabilty, in various applications including the H2S/Sour service applications. The article in the link provides an insight in welding a low sulfur material.

The issue in the context of welding is that, while sulfur content is reduced the surface tension is reduced resulting in wider concave welds with lesser penetration, which pose a problem in thick walled pipes which are common in sour services. The insert ring solution proposed in the link below may solve the problem of higher weld penetration, which calls for different weld procedure. Similar to ASME BPE standard's prescription of limitation on, weld sulfur with appropriate quality check, does such requirement called in the BPV.

I seek our member's suggestion on the subject of welding procedure qualification, in such applications where sulfur content is restricted from 0.002% to 0.010% in sour/H2S applications.

http://www.thefabri cator.com/ tubepipefabricat ion/tubepipefabr ication_article. cfm?ID=533

With regards,
Kannan

__._,_.___





--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...