Tuesday, September 29, 2009

[MW:3358] Re: Heat Input

E6010 will support up to -29 degree celcius only and used in pipe line root application. But if the PQR passes the impact you can use it with batch restriction.
regards,
Ibrahim

2009/9/29 BHARAT GOLE <bharatgole@hotmail.com>
E 7018-1 is acceptable up to -46 degree but selection E 6010 is not suitable for LTCS ! As per which clause it is selected for LTCS ?

Regards

Bharat B. Gole

 






Date: Tue, 29 Sep 2009 09:49:23 +0530
From: nach_sam@yahoo.com
Subject: [MW:3354] Re: Heat Input
To: materials-welding@googlegroups.com

Adi,
Heat input is a guideline for subsequent welding. The yardstick is the average  value as obtained from your PQR. Your production welding should not exceed PQR HI values.
By the way, is 6010, 7018-1 Ok for LTCS?  What is the working temp?
Shashank Vagal

--- On Tue, 29/9/09, Adi <adinraos@gmail.com> wrote:

From: Adi <adinraos@gmail.com>
Subject: [MW:3352] Heat Input
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Tuesday, 29 September, 2009, 9:35 AM



I have done the PQR for LTCS by using 6010 & 7018-1 as per ASME SEC IX
some time i got 5KJ heat in put
What is the limitation for heat input and where it is mention?

Adi


From cricket scores to your friends. Try the Yahoo! India Homepage!</a



Get easy photo sharing with Windows LiveT Photos. Drag n' drop





--
Thanks & Regards
Muhammed Ibrahim PK

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Dear Welding Experts, I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW +...