Hi!Noberto,

This is Normalised steel basically for Offshore structures in North sea climatic conditions
S355 J2 means 355 N/mm Sq yield strength , J2 means Impact @ -20 degrees C Avg.Impact value is 27 Joules
S355 K2 G3 means 355 N/mm Sq yield strength , K2 means Impact @ -20 degrees C Avg.Impact value is 40 Joules, G3 means Normalised Killed steel
Check dnv.com, Download this code free:DNV-OS-C401 (Mettalic materials)
SMAW process: E7018 & E7018-1
GMAW process: ER 70S-6
FCAW process: E 71T-1C/ E71T-9C

Thanks & Regards,
vipin george

On Fri, Sep 25, 2009 at 3:10 PM, Norberto Barbosa <norberto.sb@hotmail.com> wrote:
Hi, everybody
Is there someone who knows this kind of Base Material "S-355 J2 G3", regarding;
1)Similarity with ASTM;
2) Quimical Composition
3) and if possible an adequate electrode with its AWS classification and specification to weld this material.
I'll be glad.

Regardings,
Norberto de Souza Barbosa - Brazil
 





Novo Internet Explorer 8: mais rápido e muito mais seguro. Baixe agora, é grátis!



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...