Interpretation: IX-79-94
Subject: Section IX, QW-403.5 Qualification of Welding Procedure with Notch Toughness in Materials of the Same P-No. but Different Group Numbers
Date Issued: October 9, 1979
File: BC79-630
Question: Is it the intent of QW-403.5 to permit qualification of two different Group number materials within the same P-No. welded to themselves by welding one Group material to the other Group material and impact testing the heat affected zone on both sides of the weld and the weld metal?
Reply: Yes, provided the same essential variables, including electrodes of filler metals, are used when welding each base metal Group to itself.



On Mon, Nov 1, 2010 at 7:26 PM, Arunachalam A <arunvani@gmail.com> wrote:

Code Interpretations
Interpretation: IX-83-92
Subject: Section IX, QW-403.5
Date Issued: November 21, 1983
File: BC83-530
Question: A procedure has been qualified to satisfy all requirements, including notch toughness, for welding P-No.1, Gr-No.1 to P-No.1, Gr-No.1 base metals. Is it necessary to make a procedure qualification test to determine notch toughness only (QW-401.3) for welding P-No.1, Gr-No.2 to P-No. 1, Gr-No.2 base metals, with all other essential variables the same?
Reply: Yes.

Copyright Reedy Engineering, Inc. & ASME



On Sun, Oct 31, 2010 at 9:12 AM, aneesh <aneeshgopi22@rediffmail.com> wrote:

Karthik Sir,

 Is it possible to write a WPS with base metal (QW-403) P No. 1 Gr No.1  to P No.1  Gr.No.1 OR 2 ?

so possible P1GI P1G1, P1G1 P1G2 & P1G2 P1G2 Welding.

QW-403.5 is not telling to do the test again for new group no. of the same P no. material with same E&SE variables? (interpretation)

So re writing a WPS is enough for PIG1 to P1G2 welding with the current PQR  , insted of further testing ?


Please advice........... I have the same issue.

Regards
Aneesh
KSA



On Fri, 29 Oct 2010 18:36:00 +0530 Karthik karthik6684@yahoo.com wrote

Hi,

If Impact is required by Code then you have to do additional supporting PQR(CVN test only) for G2.

My interpretaion for QW403.5 as follows.


QW403.5:

If, however, two or more
qualification records have the same essential and supplementary
essential variables
, except that the base metals
are assigned to different Group Numbers within the same
P-Number, then the combination of base metals is also
qualified.


Interpreation:

As per the above highlighted sentence,If you have to PQR with CVN test of P1G1 with P1G1 and P1G2 to P1G2,then you can use this for P1G1 with P1G1, P1G2 to P1G2 , and P1G1 to P1G2 also.


In your case you have P1G1(with CVN) PQR only.So you
should do additional supporting PQR for G2.



Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.

Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282

--- On Fri, 10/29/10, Vikas Bhandari <vikas.bhandari349@gmail.com> wrote:

From: Vikas Bhandari <vikas.bhandari349@gmail.com>
Subject: Re: [MW:7929] Supporting PQR for Impact requirements
To: materials-welding@googlegroups.com
Date: Friday, October 29, 2010, 3:01 PM
Dear all

I could not find the reason to do the CVN test again for new group no. of the same P no. material. Assuming the welding process is SMAW, then as per QW 403.5, " If , however, 2 or
more qualification records have same essential and supplementary essential variables, except that the base metals are assigned to different group numbers within the same P number, then the combination of base metal is also qualified"

Pls do tell me if that is the not the case, and CVN testing is mandatory (kindly specify the relevant section from the code)
On Thu, Oct 28, 2010 at 12:34 PM, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:







Yes, you can, provided all essential/supplementary
essential variables are identical to original PQR.




From:
materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On
Behalf Of
atul chaturvedi
Sent: Thursday, October 28, 2010 4:53 PM
To: materials-welding@googlegroups.com
Subject: [MW:0] Supporting PQR for Impact requirements





Dear All,






I have Qualified PQR for welding P1 Gr 1 To P1 Gr 1 with
Impact test at (-) 51°C




thickness range 2.77 to 11.08 mm.




But now we have to weld P1 Gr 1 to P1 Gr 2. Can I do one
more supporting PQR with with P1 Gr 1 to P1 Gr 2 With only impact testing.




Please clarify whether Tensile test and bend test
aremandatoryfor supporting PQR.








Thanking you.




atul chaturvedi










--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
à®…à®°ுணாசலம்
கலைவாணி
சுதர்ஷனா
வருண்





--
à®…à®°ுணாசலம்
கலைவாணி
சுதர்ஷனா
வருண்


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...