Note: this response is directly to the question and applies only to referenced L-grade material

 

The effect on corrosion properties will be nil to minimal.

 

The use of the Low carbon (L) material minimizes any tendency towards chrome-carbide (M23C6).  For the L-grade austenitic stainless steels (3XXL) the carbon is kept below the solubility limit for carbon in solid solution.  Therefore there is little driving force to cause the formation of Cr-carbides that result in stress corrosion issues due to Cr depletion associated with elevated temperature exposures.  This is not to say that no Cr carbide may form along the grain boundaries, however if it does it will be discontinuous and will not cause corrosion problems.  Please refer to the attached generalized phase diagrams.

 

The effect on other material properties will be negligible.  The temperature is insignificant with respect to inducing structural changes.

 

There may be significant problems however with distortion of the members due to the difference in thermal expansion of austenitic alloys vs. carbon steel.  However, bear in mind that the size of the vessel  and length of the members play a major role in how much stress will be developed due to differential thermal expansion.  This may be compensated for by leaving critical connections loose enough to allow expansion and then retightening after PWHT.

 

Other than concerns with the latter point, there is no practical reason why the heat treatment could not be performed.

 

John

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of asad azmi
Sent: Wednesday, November 03, 2010 1:44 AM
To: materials-welding@googlegroups.com
Subject: [MW:8034] effect of PWHT Temperature at 600 DEG CELSISIUS ON SS 316L

 

Dear All,

 

Greetings.

 

Contractor is doing PWHT of the Carbon Steel Vessel along with  SS316L  INTERNALS ( BEAMS, CHANNELS) Bolted with the Vessel.  PWHT temperature is 600 DEG CELSIUS.

 

Pls  suggest me whether it is allowed. what will be the effect on mechanical proerties/corrosion ressiatnce  proerties of SS 316L becuase of the PWHT Temperature.

 

Thanks in advance for your valuable suggestions.

 

Regrads

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...