Try the below parameters and report back to us : 
Preheat Temperature
180°C - 200°C
Interpass Temperature
180°C - 220°C
PWHT Temperature
690°C
PWHT Duration
3-4 hours
Cooling RateSlow controlled cooling

Thanks & Regards 


On Thu, Sep 5, 2024 at 11:07 AM Prathab P <prapoovins@gmail.com> wrote:
yes, 690 degree for 2 hours.

On Sun, Sep 1, 2024 at 4:21 PM 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Is there any PWHT

Thanks & Regards

J.Gerald Jayakumar

0091-8838619635



On Sunday 1 September, 2024 at 03:24:46 pm IST, s.navaneethan.mani <s.navaneethan.mani@gmail.com> wrote:


Check the heat input reading for the test coupon.

The mechanical test reading will change If the heat input is high or low from the required values.


Regards
Navaneetha Perumal 

On Fri, 9 Aug 2024 at 9:12 AM, Prathab P <prapoovins@gmail.com> wrote:
Dear Experts,

PQR Test Coupon
Base Plate: A387 Gr22 CL2 (P. No. 5A, Gr.1)
Dimension: 500x350x40mm
Application: Heat Exchanger
Joint Design: Double Bevel

GTAW: Er90SB3
Size: 2.4mm

SMAW: E9018-B3
Size: 3.15 & 4.00mm

Preheating: 160֯C min
Interpass Temp: 200֯C max
DHT: 300֯C for 2hrs

The above mentioned test coupon impact and hardness testing failure. Impact value is getting lower and hardness value getting higher. 

The impact required average value is 55J and hardness max value is 225BHN but the impact actual value getting 22J and the hardness min actual value getting 208BHN.

What is the exert problem for this failure?

Please give us a deeper explanation for this failure. What is the solution?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFyvt4V7Gvpsaa2-01Tj63KBQW-FvqivoAD5JOA0gZj4uCD-VA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOj8udNGOp_CPoexAOdqs%3DKoxNWWqa-AoW%3D%2BtrEZo7BCGW3TXQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/129600617.1275782.1725184722132%40mail.yahoo.com.


--
Thanks and Regards

P. PRATHAB
+91 9159743943

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFyvt4XQLkbko5mLnuJ%3DJCyrvrfrw5maHkRuoHXjpgK7W%3DH%2B4A%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFhOWxY%2B%2BD_Mrk-zNjB8nbZm5Ydyv9R3U71ZnCwLGsrE-ENb%3Dg%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...