Skip to main content

Re: [MW:33536] Production Test Plate

Please also consider thickness & welding process.

Thanks & Regards

J.Gerald Jayakumar




On Tuesday, 4 October, 2022 at 03:32:22 pm GMT+4, Sourav Bohrays <souravbohrays@gmail.com> wrote:


for thickness less than 10mm -300x350mm 
  thickness more than 10mm-300x400mm
PTC should be as per each wps used as per each seam.
if wps same for cat A and Cat B -1 ptc require
if wps use for dish head is same as cat A and B no ptc require extra
if wps use for dish head is diff as cat A and B  ptc require separate
refer below attach pic also
image.png


On Tue, 4 Oct 2022 at 16:36, williams p wilson <williamswilsonp@gmail.com> wrote:
Dear Gerald Sir,
Greetings!!

Please advise the dimensions of the test plate.
300 mm (W) x 500 mm (L) is enough.

In our case one test plate is required for each welding procedure used for Cat. A & B Joints. 
80 mm thick dish heads are manufactured with a single joint - PTC is required for these joints.

Thank You & Regards
Williams P Wilson
+968-94600828
QA/QC Engineer
Please consider the environment before printing this message


On Tue, Oct 4, 2022 at 1:14 PM Sezgin Ckllı <euniversty@gmail.com> wrote:
Thank you Mr. Gerald.

Believe me, you've been very helpful.

Thanks & Regards

Sezgin ÇAKALLI


4 Ekim 2022 Salı tarihinde saat 06:20:02 UTC+3 itibarıyla gerry_tup şunları yazdı:
Figure (1)

Weld (Thickness 15mm)

1 set with notch in the weld 1.5mm from the top surface (SAW Process)
If GMAW weld metal greater than 2.5mm, 1 set in GMAW weld subsize

HAZ

1 set from  1/4t to 1/2t in SAW  HAZ
If GMAW weld metal greater than 2.5mm, 1 set in GMAW HAZ subsize


Figure(2) 50mm

Weld

1 set 1.5mm from the surface with the notch in the SAW weld
1 set below the GMAW weld in the SAW weld near to centerline and notch in SAW weld
If GMAW weld metal greater than 2.5mm, 1 set in GMAW weld subsize

HAZ

2 sets in HAZ as per table 84.6
If GMAW weld metal greater than 2.5mm, 1 set in GMAW HAZ subsize


Figure (3) 35mm

Weld

1 set with notch in the weld 1.5mm from the top surface (SAW Process)
1 set with notch in the weld 1.5mm from the root surface (GTAW Process)subsize


HAZ

2 sets in HAZ as per table 84.6
If GTAW weld metal greater than 2.5mm, 1 set in GTAW HAZ subsize




Thanks & Regards

J.Gerald Jayakumar


On Monday, 3 October, 2022 at 02:43:51 pm GMT+4, Sezgin Ckllı <euniv...@gmail.com> wrote:


That's why we subjected it to the impact test.
What I want to learn is how many samples should be taken from where in the sourced material I want to specify below?

P.T. -1_ASME-WPS-22-06_1_GMAW+SAW_15mm.jpg

P.T. -1_ASME-WPS-22-06_1_Rev1_GMAW+SAW_70mm.jpg

P.T. -1_ASME-WPS-22-01_1_Rev1_GTAW+SAW_30mm.jpg

I will be glad, if you inform me.

Yours truly

3 Ekim 2022 Pazartesi tarihinde saat 12:43:30 UTC+3 itibarıyla gerry_tup şunları yazdı:
When Impact testing is a design requirement as per ASME Sec.VIII Div.I, production Impact testing is required. Only Impact test is the requirement as per ASME Sec.VIII Div.I unless other tests are required by your Client Requirement.


For production Impact test follow below section.

Inline image

For any specific requirement as per below table, please describe in detail what clarification you require.

Thanks & Regards

J.Gerald Jayakumar


On Monday, 3 October, 2022 at 12:05:30 pm GMT+4, Sezgin Ckllı <euniv...@gmail.com> wrote:


Thank you Mr. J. Greald 

But as far as I have learned, please pay attention to the following paragraph and confirm its accuracy.

** resim_2022-10-03_103603900.png
Regards 

Sezgin ÇAKALLI
3 Ekim 2022 Pazartesi tarihinde saat 07:43:02 UTC+3 itibarıyla gerry_tup şunları yazdı:
UG-84

Thanks & Regards

J.Gerald Jayakumar




On Monday, 3 October, 2022 at 08:22:28 am GMT+4, Sezgin Ckllı <euniv...@gmail.com> wrote:


We design a pressure vessel according to ASME VIII Div.1 and our customer request shows "Production test plates according to Code requirements". Can you tell us the section showing where we can take samples from materials that vary according to their thickness. Or I need someone to contact me about the issue.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/3ff85526-0de0-44a3-b2f3-6ec89fe81124n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/e38ad76c-ec2e-41fb-96a0-073cdcb02d10n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHBxnQ7B%3DJRnAO5%2BG8kCSn6sU6TKuYKoqeTgBmEnfkR62Zqzow%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOWr6k_ZbnnWf5ixSSD5eW28r6TsF8ZrAcd79n-EM7MD7o8O3w%40mail.gmail.com.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...