[MW:33588] RE: 33587] Black dots on sdss welding

Hi Narayanan,

 

Please refer the discussions and the answers provided the following link. The spots may appear due to few issues:

  • Type of lubricants used during wire drawing of the GTAW filler wires. Typically oil based lubricants if used could generate such residues, while soap type lubricants  may not.
  • Surface finish of the SDSS. If the products are acid cleaned & pickled after manufacturing the chances of such welding dross would be less.

Irrespective of those facts, the discussions in this following link are worthwhile to look at.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

Black spots on DSS Weld Joints. (google.com)

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Narayanan Kumar
Sent: October 11, 2022 9:31 AM
To: materials-welding@googlegroups.com
Subject: [MW:33587] Black dots on sdss welding

 

Dear Team,

 

Can you please explain about the black dots appears on SDSS GTAW Weld bead( ER 2594 )  with document backup for the causes 

 

 

Regards,

 

M.Kumar 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADTvyj%2B9Ti77s60HeABOGGgrcOeok0BG2nwCqMQQ8zrDqdyGyw%40mail.gmail.com.


Virus-free.www.avg.com

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...