Re: [MW:29502] Aluminium Bronze welding

You can maintain flow rate of argon gas @ 15 LPM.

Regards

Prem Nautiyal


PREM S NAUTIYAL
CELL : 9769316004





From: Mohammed afzal Khateawdi <afzal8880@gmail.com>
Sent: Sun, 21 Apr 2019 18:58:51 GMT+0530
To: materials-welding@googlegroups.com
Subject: Re: [MW:29500] Aluminium Bronze welding

Hi....Prem 

Hereafter considering below points as per you, Plz share with us what was flow rate l/min for Argon gas ?

Use 99.995% pure argon

Preheat 150 – 180 ˚C

Inter pass temperature @200 ˚C

Inter run cleaning is very important to remove surface oxides 

Thanks & Regards,




On Tue, Oct 2, 2012 at 6:51 PM prem nautiyal <prem_nautiyal26@yahoo.com> wrote:
Hi
 
Why dont you read the subject line and the past discussions before posting your query ?
We are discussing Aluminium bronze. Dont create confusion ..
 
Regards
 
Prem Nautiyal


--- On Tue, 10/2/12, Ashish Pathrabe <darkash6633@gmail.com> wrote:

From: Ashish Pathrabe <darkash6633@gmail.com>
Subject: Re: [MW:15444] Aluminium Bronze welding
To: materials-welding@googlegroups.com
Cc: "kannayeram gnanapandithan" <kgpandithan@gmail.com>
Date: Tuesday, October 2, 2012, 1:25 PM

Dear Esperts:=
 
You are replying for Aluminium Bronzee or for monel Welding.
 
pls , clear the confusioo
 
Ashishj

On Sun, Sep 30, 2012 at 9:14 PM, prem nautiyal <prem_nautiyal26@yahoo.com> wrote:
No doubt Helium+Argon mixture will give better fusion and penetration, but i have welded lot of Al-Br with Pure argon.
Hel+Ar mixture is a costly affair.
Also preheat is must.
 
Regards
 
Prem Nautiyal


--- On Sun, 9/30/12, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:

From: kannayeram gnanapandithan <kgpandithan@gmail.com>

Subject: Re: [MW:15374] Aluminium Bronze welding
To: materials-welding@googlegroups.com
Cc: prem_nautiyal26@yahoo.com
Date: Sunday, September 30, 2012, 1:13 PM


use helium+argon mixture
need not preheat
clean properly
pandithan
In-charge/wt
Cethar

On 9/24/12, bo gyi <aungbomyint@gmail.com> wrote:
> Hi
>
> Base material is B171 C61400 & 99.9995% argon is used.
>
> Regards,
>
> On Friday, September 21, 2012 10:01:11 PM UTC+8, prem nautiyal wrote:
>>
>>
>> Hi
>>
>> Its not an easy task to weld Al bronze.
>> What is your base material grade ?
>> Clean base metal and filler wire before welding.
>> Use 99.995% pure argon.
>> •Preheat 150 – 180 ˚C
>> •Inter pass temperature @200 ˚C.
>> •Inter run cleaning is very important to remove surface oxides
>>
>> Regards
>>
>> Prem Nautiyal
>> Cell: 9769316004
>>
>> --- On *Fri, 9/21/12, bo gyi <aungb...@gmail.com <javascript:>>* wrote:
>>
>>
>> From: bo gyi <aungb...@gmail.com <javascript:>>
>> Subject: [MW:15353] Aluminium Bronze welding
>> To: material...@googlegroups.com <javascript:>
>> Date: Friday, September 21, 2012, 7:46 AM
>>
>> Hi Sirs,
>>
>> Currently, I am doing procedure for Aluminium Bronze (61400) using GTAW (
>>
>> ERCuAl-A2) process by Argon shielding gas but found that fusion of filler
>>
>> metal & base metal is not nice.
>>
>> Can anyone advice?
>>
>> Thanks and regards,
>>
>> Bo
>> --
>> To post to this group, send email to
>> material...@googlegroups.com<javascript:>
>> To unsubscribe from this group, send email to
>> materials-weld...@googlegroups.com <javascript:>
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>>
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views and
>>
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>>
>>
>>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
>
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https:roups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...