In my opinion No preheating, Aluminum oxide will form,breaking may be the reason . Try without preheating.
On 08-Dec-2017 4:09 PM, "Sathish Kumar" <sathishmech04@gmail.com> wrote:
Dear Experts
I need query on Aluminium welding
Material -6061-T6
Material Thickness-16mm
Filler wire- ER4046
Process-GMAW
Pre heat-70 centigrade
Interpass- 120 centigrade
Preclean by Acetone cleaner and SS wire brush
Gas-Ulta high purity Argon gas
During PQR qualifications we face failure in bend test. Crack open at 30degree itself. Is the above method required PWHT after welding. If so what is the method of PWHT and cycle.
Kindly clarify?
Thanks in advance
Regards
Sathish
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Comments