Re: [MW:26481] Welding of aluminum 5083

Yes,u can,but use He75%+Ar25%. Clean thoroughly while fit up and before start of welding.

On 26-Apr-2017 4:08 PM, "Hani Al Masry" <hanyonalfy@gmail.com> wrote:
Yes exactly but it's not available in UAE
I will use instead 5356 1.6mm?
Also what should do to concert the machine to GMAW?
Can you send me WPS?

Regards
H.A

On Apr 26, 2017 2:19 PM, "Kannayeram Gnanapandithan" <kgpandithan@gmail.com> wrote:
5183

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Apr 25, 2017 at 8:32 PM, Hani Al Masry <hanyonalfy@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (hanyonalfy@gmail.com) Add cleanup rule | More info

Dear all

We have aluminum 5083 tank which have some small hopes in shell plates 
We prefer to go for injection wields to close these hopes 
Holes are in 5 mmm diameter 

Can you advice procedures and electrode to be used?

Regards 
HA

On Mar 17, 2017 3:33 PM, "Hani Al Masry" <hanyonalfy@gmail.com> wrote:

Dear All

Please advice we have to fabricate some pulling heads from pipes grades 
X60 and X65 with plates grade S355 

We proposed WPS for welding of X65 as the higher grade to be covered also for X60 and for S355 

Is these WPS 's are enough?or we need other?

HA
Regards

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKOkEzfEQx73UVqQGT98%2BzCXR356MFtQTaWfZNh0NsKv6vQjew%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNK-iC8k%2Bm9P3a5qCjTm4zbEm1yKe%3DUjBnYbg_jYegswQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKOkEzfTaqnAZpz3Ci5EvJ-OH5nZJ7RENAfsrfCbnsxZm8zqYw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4ePdQxHNcU%2Bpjrn%2BMt3%2BYyu1JOMrtPCWHAgzPnXjHQ0CNg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...