Re: [MW:26397] Re: Welding of ASTM A 335Gr.P11

Dear sir, 

   Thanks for your valuable reply, actually we are not going to use ER-90SB9 & E-9018B9, CHINESE  proposed to do weld with ER-90SB3 & E-9018B3. for this please suggest me what temperature have to give for soaking and holding time. for your valuble reply i'm awaiting sir.

Thanks & Regards
M.SAI PRATHAP
assistant manager(QA/QC)
IPCL, INDIA
  

On Wed, Apr 12, 2017 at 12:33 PM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
There will be depletion of C and Hardness also will increase if u use ER90S-B9 and E9018-B9 and soaking time of P11 will not reduce much of Hardness of B9 weld metal

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Apr 12, 2017 at 8:55 AM, prathap sai <sai.prathapmv@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (sai.prathapmv@gmail.com) Add cleanup rule | More info

Dear sir,

  Thanks for your valuable  reply, i also suggested the ER-80SB2 & E-8018B2 for welding of P11, but the chinese has saying that,they will use ER-90SB3 & E-9018B3 instead of ER-80SB2 & E-8018B2 . Till now QPS & PQR also not prepared.for that reason only i asked here. i have to approve the proposed WPS. please let me know the soaking temperature have to given when ER-90SB3 & E-9018B3 used for P11.Is there any effect on the hardness values when we will give soaking temperature of P11.

Thanks & Regrds
M.SAI PRATHAP
assistant manager(QA/QC)
IPCL, INDIA

On Tue, Apr 11, 2017 at 5:19 PM, 'Sankaran Sp' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Friend,

For  welding of SA335-P11 pipe you can use ER-80S-B2 & E8018-B2 for welding, no need to use 
ER-90SB3 & E-9018B3. 
For PWHT you can use 650-660 Deg C with soaking time respect to thickness of job or refer ASME secVIII div 1 standard.
Hope that i have clarified. 

Regards,
Sankaran.SP
welding& metallurgy expert     


On Tuesday, 11 April 2017 2:50 PM, sai prathap <sai.prathapmv@gmail.com> wrote:


Dear sir,

  i'm having one doubt that, can i use ER-90SB3 & E-9018B3 for welding of SA335-P11. if suppose will use then what is temperature should have to follow for the PWHT. if we follow the soaking temperature of P11, then is ther any chance to affect on the hardness properties.

Thanks & regards
M.SAI PRATHAP
+91-8332897606

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/07d51d40-3b4c-4a6d-bf0a-c3afc9f13df1%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/q9d2jvitCn8/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/736214644.247374.1491911377297%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANaej0ehHUadbo1ZxaNhwbxNL%2BEShVX5wf%2BEqBwrNE0BkoHu7w%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to a topic in the Google Groups "Materials & Welding" group.
To unsubscribe from this topic, visit https://groups.google.com/d/topic/materials-welding/q9d2jvitCn8/unsubscribe.
To unsubscribe from this group and all its topics, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eP62U%3DSL7OsSkNASjeei%2B%2BgLvD2H8SdxwhGO5rP8Bo4Lg%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANaej0e4EUs9Sy_q%3DOt-mtiiMmpxWi28KDTCvAYaQ821OxodSw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...