Skip to main content

[MW:26398] Re: ASME Sec VIII Div.1 UCS-79 clarification

Dear All,

I would like to ssek your advice on the following:

As per project specification ,All parts which have been cold formed with an extreme fiber elongation greater than the following shall be subjected to the following heat treatment:  

Carbon and low alloy steels, 5% normalizing and tempering treatment.

 

Currently the purchased plate is a carbon steel with which is already in normalized condition.

 

Our vendor is asking not to perform tempering because as advice from the mill,they cannot guarantee the plate mechanical properties after tempering since the plate supplied in Normalized condition.Vendor will only perform Normalizing Heat Treatment for the plate.


Since i'm not expert,anybody having any experience or knowledge on this can advice me.


Thanks


On Wednesday, September 5, 2012 at 7:14:41 PM UTC+2, prem nautiyal wrote:
Hi friends
 
A vessel is being fabricated as per ASME Sec VIII Div.1.
MOC is SA 516 Gr.70
The 2:1 ellipsoidal Dish end nominal thickness is 16mm / min thk 14mm. There is no PWHT and Impact test requirements in the vessel.
I would like to know whether this 16mm thk dishend requires stress relieving or not as per UCS-79.
Vendor has offered dish ends without SR. Is it acceptable?
Nothing is mentioned in client specs and drawing about D/E SR.
 
Regards
 
Prem Nautiyal
 
 
 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bcd6f52a-a852-45dd-b94e-28e6670678a8%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...