Skip to main content

RE: [MW:25990] WELDER QUALIFICATION CERTIFICATE RENEWAL AS PER ASME SEC. IX

Hi Manoj,

You can renew the qualification of a welder as per clause QW-322.1 a) (1) of ASME Section IX: 2015 Edition, ie. If a welder works continuously under the supervision and control of the certifying personnel / organisation, his qualification will be extended for another 6 months without any NDT reports, weld visual report is enough.

I believe the above is in order, I request experts kindly interprate above and correct me if I am wrong.

Regards 
Govindan P







Jan 26, 2017 19:36, "John Henning" <jhenning@deltak.com> wrote:

What your customer is demanding is different than what the Code requires.  There is NO requirement in ASME Section IX that the weld be inspected in any way, volumetric or otherwise.  The requirement is to only to determine that the process was used by the welder.

 

Other Codes, EN in particular, require that the weld used for prolongation of qualification be volumetrically examined.  This NOT required by ASME Section IX.

 

If you are fabricating in accordance with an ASME Code and using Section IX for qualification, then the issue is contractual, i.e. solely between the fabricator and customer.  Just because your customers are specifying a requirement does not make it a Code requirement.

 

While there may be some justification for such a requirement, it becomes a logistical nightmare and just another reason why European fabrication is outrageously expensive.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of vinay yadav
Sent: Wednesday, January 25, 2017 4:30 AM
To: Materials & Welding
Subject: Re: [MW:25984] WELDER QUALIFICATION CERTIFICATE RENEWAL AS PER ASME SEC. IX

 

GOOD AFTERNOON ALL,

 

 

MY CONCERN IS HOW WE WILL TRACE THE RADIOGRAPHY CARRIED OUT ON WELD IS OF SAME WELDER WHICH WE QUALIFY ?


REGARDS,
VINAY

 


On Wednesday, January 25, 2017 at 2:21:27 PM UTC+5:30, John Manoj wrote:

Thanks for your reply,

but what is the proof we can provide for his continuity of welding, always everybody is asking radiography report.  RT reports or any other NDT reports may not be available in some cases, like fillet weld.  

 

On Sat, Jan 21, 2017 at 4:18 PM, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:

As per ASME IX, Renewal only for qualified Welding Process, with fillet weld u can 


THANKS & BEST REGARDS,

KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,

CONSULTANT-WELDING & QUALITY

Mobile no: +919940739349

 

On Sat, Jan 21, 2017 at 2:42 PM, Manoj John <manoj...@gmail.com> wrote:

BoxbeThis message is eligible for Automatic Cleanup! (manoj...@gmail.com) Add cleanup rule | More info

 

Dear Friends,

 

We have qualified welders in groove welding (GTAW+SMAW) as per ASME section IX but they have welded 2 months butt welding and 4 months they welded only fillet joints. Now they completed 6 months and they are continuing welding.  

 

My question is how can we renew their certificates since they do not have any Radiography reports for fillet joints.  Can we renew their certificate with a visual inspection report.

 

Thanks & Regards.

 

Manoj John.

 

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACgUO5nBM2QU9Uv6y98y1YLy0gpA8sbUU88XHKG0LHHaeEnZ%3Dw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eO2O_Qf68KQY%3DeYCJnSfq-HZ%3DdMg2j2HVTiNMC0gwzvrA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c295cef6-70f0-47c1-ba44-455ccb106580%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/MWHPR03MB28166BE1C32386C0B2E393F7A1770%40MWHPR03MB2816.namprd03.prod.outlook.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANiuf9eJJT94JEvr56u2EAAWb80oRfeA5abLhDQo8hGiLX5hzA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...