Skip to main content

RE: [MW:25959] Fillet size a6 with single layer (GMAW welding process)

Ok,
Sure I will try the on given parameters and I will update you all with macro graph.
Thanks for your support.
Vijay Katkar.

On 20 Jan 2017 9:33 p.m., "pgoswami" <pgoswami@quickclic.net> wrote:

Hello Vijay,

 

To answer to your query in a straight forward language:-

  • Depositing a fillet weld of 6 mm throat by GMAW process in a single pass is difficult. 6mm of throat = 9 mm of leg length, which is difficult to cover in one pass, unless the welder does edge to edge weaving.
  • Extended weaving would cause  loss of  travel speed and  production time.
  • Also it would induce undue defects e.g. toe undercuts. If so, one has to spend more time on grinding and subsequent dress ups, a redundant exercise.
  • Also if the materials have notch toughness or corrosion resistance requirements ( for austenitic or other stainless steels) , it may be compromised by a single pass technique.
  • Hence the so called gain of production time would mean nothing.

 

The parameters suggested by you are fine, if you perform a multi pass techniques. Or else you may try the welding parameters suggested by Mr Kannayeram Gnanapandithan, however the welder has to be comfortable. If the fillet weld involves any more welding positions other that 1F, 1.2 mm dia filler is more flexible to weld with.

 

Thanks.

 

 

 

Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineering Specialist.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannayeram Gnanapandithan
Sent: Friday, January 20, 2017 9:23 AM
To: materials-welding
Subject: Re: [MW:25956] Fillet size a6 with single layer (GMAW welding process)

 

Use 1.6mm, amp around 355

 

On 16-Jan-2017 10:12 am, "Vijay Katkar" <katkar.vijay22@gmail.com> wrote:

Dear Experts,

 

Our customer is forcing us to do multilayer welding for 6mm throat size, which is increasing our welding time because most of welding is in a6 size.

 

I have tried so many test coupon to prove that a6 can be done by single layer but I am not succeed in all test.

 

Customer requirement is root penetration at least 0.3 mm. But I am not able to achieve it. refer following parameters which I have used.

 

  • Welding process :- GMAW
  • Filler Wire :- ER 70 S6 (1.2 mm dia)
  • Shielding gas :- 80 % Argon + 20 % Co2
  • Current :- 245-255 Amp
  • Voltage :- 26.5 to 27.5
  • Travel speed :- 220 - 240 mm/min

Please advise any modification is required in the parameters.  

 

Should I change Shielding gas composition?

 

Waiting for your valuable reply?

 

Thank you

 

Vijay Katkar

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAP37wrKnxUoYE9r4ACS5vgf2Yo1UWw3MqJD25Khyw9LJDMG1Tw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNnuo8h7GBukApQOm-porkj8PRk%2BMeJYg6sSrALXSqSaA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!~!UENERkVCMDkAAQACAAAAAAAAAAAAAAAAABgAAAAAAAAA5rYMdESrHU2r7z2aNylU0sKAAAAQAAAAbbB0O9/5lk2Brcj79yieigEAAAAA%40quickclic.net.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAP37wrJQSBfbc5mUwvP73z_4WZ-Fhk9WasCw%3DeobFyBTD%2BXqog%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...