Re: [MW:24984] P8 material WPS to comply QW 407.2_PWHT temperature_time

You have to read QW-407.1. 
according to this paragraph for P-number 8 it is up to you to define the "specified temperature range". So, remember that ASME BPVC is not a Handbook and look in the bibliography what is the acceptable temperature range for solution annealing

2016-06-19 20:59 GMT+03:00 Praveen Kumar <praveenkumar.tkm@gmail.com>:
Dear Mani

If you have impact requirements the clause 407,2 also applies , in that case  the requirement of new pqr is needed. 
Secondly the long soaking time of 7 hours , will have some deteriorating effect on ASS, Kindly check that also. 

On Saturday, June 4, 2016 at 10:06:18 AM UTC+4, jaya anil wrote:
In this case , you need to qualify new PQR. 

Read ASME Section IX QW 407..clauses.

On Sat, Jun 4, 2016 at 5:49 AM, manivannan hemu <hemuman...@gmail.com> wrote:



Dear All,


I have a Query.


We have a SMAW-WPS [ASME SEC IX] for material P8/G1 – PQR with CHARPY tested. In this PQR it was post weld heat treated to re solution anneal at 1090 DEG C for 2 Hrs.


Now we have new production weld requirement  on a part of 8 inch thick with PWHT [solution anneal] at temperature 1130 DEG C and soak time of 7 hrs.


Please clarify me, is it acceptable to revise the WPS [with the same PQR] to address PWHT temperature as 1130 DEG C, and time as 7 hrs to utilize for the new production weld.


In doing this I considered QW407.1(b) (2) 'PWHT within specified temperature range' – in this case specified temperature range for solution anneal as 1040 DEG C minimum by ASTM A351, and NO maximum is specified.


I appreciate your response with the intent requirement of QW 407.2


Regards, MANIVANNAN.P

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5432c488-6730-400a-8abc-0ef4a78db4d3%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f882c533-7856-479d-921f-be4c9695c0f3%40googlegroups.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CxeYmGfmSW3-jEVSd9b5jW2jFj-Gt1Bgd%2BXSWGRmrXtA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...