Skip to main content

Re: [MW:24984] IMPACT TEST REQUIREMENT

No, if you read carefully the last sentence of 5th paragaphe of QW-403.5 the combination in the same test coupon qualifies the group numbers to themselves.
However if the application Code Section (VIII-1, VIII-2) does not require HAZ impact testing you dont have to worry about this variable

2016-06-18 12:11 GMT+03:00 'Mohammed Rafiuddin' via Materials & Welding <materials-welding@googlegroups.com>:
PQR on P1Gr1 to P1Gr2 qualifies welding P1Gr1 to P1Gr2 only and NOT welding to themselves i.e ( P1Gr.1 To P1Gr1 Or P1Gr2 to P1Gr2)

Refer ASME interpretation IX-92-70 on the same subject.I could not find downlodable copy.Try to search on internet.

Thanks
Mohammed


On Friday, 17 June 2016 1:52 PM, "nithindsilva4u@gmail.com" <nithindsilva4u@gmail.com> wrote:


P1 G1 to P1 G2 qualifies P1 G1 to P1 G2, P1 G2 to P1 G2 and P1 G1 to P1 G1. Hope your query is addressed.

Sent from my iPhone

On Jun 17, 2016, at 11:37, balaji srinivasan <bolukbalaji@gmail.com> wrote:

Dear All,


As per ASME SEC-IX   change in material Group is Supplementry  essential variable (403.5)

based on above i need your experience  If iam qualified PQR p1 group-1 to p1 group-2 tow different group welded it self so the  qualfied range will be p1 group1 and p1 group 2.

or only this PQR is qualified group 1 to group-2 qualified.

also please advice i need to qualify group 1 separate and group 2 separate PQR.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAK1csg3Drkobg2%3DG9Lyy0CMd3WbM%2BOq_9e2GkJLoC-QxBUhP0A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0232776F-14AF-4FF0-8B7E-DA998585BF07%40gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/492345405.4017979.1466241063907.JavaMail.yahoo%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CAYkD_Ub6S4gpgeFS-a4yyb_rZ4VaDSAvsMkev514APQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...