Skip to main content

Re: [MW:24970] IMPACT TEST REQUIREMENT

PQR on P1Gr1 to P1Gr2 qualifies welding P1Gr1 to P1Gr2 only and NOT welding to themselves i.e ( P1Gr.1 To P1Gr1 Or P1Gr2 to P1Gr2)

Refer ASME interpretation IX-92-70 on the same subject.I could not find downlodable copy.Try to search on internet.

Thanks
Mohammed


On Friday, 17 June 2016 1:52 PM, "nithindsilva4u@gmail.com" <nithindsilva4u@gmail.com> wrote:


P1 G1 to P1 G2 qualifies P1 G1 to P1 G2, P1 G2 to P1 G2 and P1 G1 to P1 G1. Hope your query is addressed.

Sent from my iPhone

On Jun 17, 2016, at 11:37, balaji srinivasan <bolukbalaji@gmail.com> wrote:

Dear All,


As per ASME SEC-IX   change in material Group is Supplementry  essential variable (403.5)

based on above i need your experience  If iam qualified PQR p1 group-1 to p1 group-2 tow different group welded it self so the  qualfied range will be p1 group1 and p1 group 2.

or only this PQR is qualified group 1 to group-2 qualified.

also please advice i need to qualify group 1 separate and group 2 separate PQR.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAK1csg3Drkobg2%3DG9Lyy0CMd3WbM%2BOq_9e2GkJLoC-QxBUhP0A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0232776F-14AF-4FF0-8B7E-DA998585BF07%40gmail.com.
For more options, visit https://groups.google.com/d/optout.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .