Re: [MW:24286] Alloy Material P22, A335 (Cr2.25 and Mo 1)

Dear Bhatti,

Your actual answer is yes. You have to do PWHT as your WPS is qualifies with PWHT (essential variable). 

You have an option:

You can avoid PWHT.............if your construction code is ASME B 31.3.
1st you have to qualify an WPS without PWHT.
2nd: for production weld you have to do recommended preheat as per WPS.
And please make sure the piping service does not fall under the following services: (Check your Piping Material Specification)
a. NaOH
b. MEA
c. DGA
d. ADIP
e. Hydrogen
f. DEA
g. MDEA
h. Boiler Deaerator.
i. Sour

If your service falls under the above services you have to do PWHT for your cases.

Regards

On Sat, Feb 13, 2016 at 5:01 PM, 'nawab ali bhatti' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Sir

Thanks for reply
Shoe support material is P22 / A335 thickness 12 mm and WPS qualified with PWHT 

Best Regards



From: 'Biplab Pal' via Materials & Welding <materials-welding@googlegroups.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Saturday, February 13, 2016 1:47 PM
Subject: Re: [MW:24279] Alloy Material P22, A335 (Cr2.25 and Mo 1)

Dear Bhatti,

First you tell me what is the material you have selected to use as a support and what is the thickness for the support material.
If your WPS is qualified with PWHT you have to do the PWHT.
If PWHT is service requirement you have to do PWHT.
Other cases you have to follow construction code (unless otherwise specified in client std/specification).

Regards


On Thu, Feb 11, 2016 at 8:09 PM, 'nawab ali bhatti' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear Experts

Please   share your best  experience  with reference of international codes

Pipe Material  P22, A335 (Cr2.25 and Mo 1), Shoe support to be welded direct with pressure parts.(Pipe material thickness 33 mm, Operating Temperature 500 Centigrade  and pressure 106 bar)
 
My question,   Is  PWHT require for shoe supports  Or Not???
                     Shoe support plate thickness is 12 mm and throat thickness is 8 mm, Preheating is perform as WPS.


NA Bhatti
00966 593530001



                     
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/241801168.2167526.1455201549003.JavaMail.yahoo%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.



--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   biplab.mech@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFnzQg0ngBL_c-qocJPESONCNndxEg1weQoV6qD6Du0TbJzeow%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2112418457.2906144.1455363063712.JavaMail.yahoo%40mail.yahoo.com.

For more options, visit https://groups.google.com/d/optout.



--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   biplab.mech@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFnzQg2VfSnssoxPDpWWrnyYxbuPadRnqT4uwu7BJ8MYu5me0A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...