Skip to main content

Re: [MW:23596] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

Correct.
Any way contact with carbon steel, copper and chlorides must be prevented

Sent from my BlackBerry 10 smartphone.
From: elias jarjoura
Sent: Τρίτη, 29 Σεπτεμβρίου 2015 - 11:06
To: materials-welding@googlegroups.com; Neilash Kumar
Reply To: materials-welding@googlegroups.com
Subject: RE: [MW:23590] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

1 -Should try passivization after pickling 
Nitric Acid Passivation of Stainless Steels
—Chromium-Nickel Grades (300 Series)
—Grades with 17% Chromium or more (except 440 Series)
20% by vol. nitric acid at 120/140°F (49/60°C) for 30 minutes
—Straight Chromium Grades
   (12-14% Chromium)
—High Carbon-High Chromium Grads (440 Series)
—Precipitation Hardening Stainless
20% by vol. nitric acid + 3 oz. per gallon (22 g/liter) sodium dichromate at 120/140°F (49/60°C) for 30 minutes
or
50% by vol. nitric acid at 120/140F (49/60°C) for 30 min.

Passivation is a post-fabrication method of maximizing the inherent corrosion resistance of the stainless alloy .

2 -Painting option :


a)surface preparation :

Abrasive blasting can be accomplished by using clean, fine, hard non-metallic abrasive particles (e.g. alumina or silicon carbide). The abrasive medium must be iron-free to avoid contamination, which can result in rust staining on the surface prior to coating and the compressed air carrying the abrasive medium must be free of compressor oil.

b) Prior to coating, all stainless steel surfaces must be dry and free from rust, other foreign materials, oil and grease. The presence of such contaminants may lead to failure of the coating system.

c) coating application and system 

he table below gives details of paint systems suitable for coating stainless steels and, in accordance with ISO 12944 and ISO 9223, classifies them in terms of the severity of the envisaged service environment.


Exterior EnvironmentCoating System
CategoryCorrosion RiskLocation.
C3MediumRural and urban areas with low sulphur dioxide, acid, alkali and salt pollutionTwo pack epoxy or polyurethane primer suitable for stainless steel at 30-50 micron dry, FOLLOWED BY High solids polyurethane finish at 100 micron dry
C4HighUrban and industrial areas with moderate sulphur dioxide and/or coastal areas with low salinityTwo pack epoxy or polyurethane primer suitable for stainless steel at 30-50 micron dry, FOLLOWED BY High build epoxy MIO* at 100 mm dry, FOLLOWED BY Re-coatable polyurethane finish at 60 micron dry
C5IVery HighIndustrial areas with high humidity and aggressive atmospheresTwo pack epoxy or polyurethane primer suitable for stainless steel at 30-50 micron dry, FOLLOWED BY High build epoxy MIO* at 200 micron dry (one or two coats), FOLLOWED BY Re-coatable polyurethane finish at 60 micron dry
C5MVery HighCoastal and offshore areas with high salinityTwo pack epoxy or polyurethane primer suitable for stainless steel at 30-50 micron dry, FOLLOWED BY High build epoxy MIO* at 200 micron dry (one or two coats), FOLLOWED BY Re-coatable polyurethane finish at 60 micron dry

MIO = Micaeous Iron Oxide

Cleanliness is extremely important in the successful application of paint coatings to stainless steels surfaces. Paint coatings should be applied in clean, dust-free conditions to clean, dry stainless steel surfaces.

If the correct precautions are taken, the complete coating systems suggested in the table can be applied in 'on-site'.


Best Regards 

Elias 




Subject: [MW:23584] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD
To: neilashkumar@yahoo.com
CC: materials-welding@googlegroups.com
From: george.dilintas@gr.bureauveritas.com
Date: Tue, 29 Sep 2015 10:04:06 +0300

It looks like iron contamination.
Actions to implement:

  1. Removal of rust by stainless steel compatible brushes/disks.
  2. Pickling
  3. Avoid contact with carbon steel tools, jigs etc

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Inactive hide details for Neilash Kumar ---29/09/2015 09:56:39--- Dear Sir, Good Morning, please find the attached tank drawingNeilash Kumar ---29/09/2015 09:56:39--- Dear Sir, Good Morning, please find the attached tank drawing

From: Neilash Kumar <neilashkumar@yahoo.com>
To: George H Dilintas/GRC/VERITAS@VERITAS, Welding Groups <materials-welding@googlegroups.com>
Date: 29/09/2015 09:56
Subject: NEED ADVISE CORROSION IN INHIBITOR TANK REGD




 Dear Sir,

Good Morning, please find the attached tank drawing
fabricated by us for our client & it is corroded fully ,
Can you please clarify,
1. Why the tank are corroded So fast?
2. Can you please advise us the method to stop /reduce the rate of corrosion by applying a top coat &  what
type of coating to be applied?

please advise me . Material is 316L tank.

Regards
P.Neilashkumar[attachment "20150909_102338.jpg" deleted by George H Dilintas/GRC/VERITAS] [attachment "20150909_102358.jpg" deleted by George H Dilintas/GRC/VERITAS]

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/OF5C1CA9F0.D638C881-ONC2257ECF.0026A74C-C2257ECF.0026D431%40LocalDomain.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/DUB113-W681E878F368E29B9EF85298A4E0%40phx.gbl.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...