Skip to main content

Re: [MW:23514] Re: SURFACE DEFECT IN HOT ROLLED PLATES

I think these plates are stacked one over the other in open yard, probably in sea port. During night, the moisture condenses on the edges and slowly flows inside. Causing this type of surface corrosion.

2015-09-23 12:50 GMT+04:00 Mattia Degli Esposti <mat.degliesposti@gmail.com>:
Dear Mehdi Vafakhah,

I try to response to your question with a low number of informations. So I can make an assumption: the material has no defects, like segregation and wrong chemical composition.
In this point of view, the reason of these defects is searchable in hot rolling parameters. Especially analyzing the photo 22222.jpg, it's clear that the metal couldn't follow the plastic deformation imposed by the process. So in my opinion defects are due to:

-  temperature too low
-  strain rate too high (attributable to an angular velocity of rolling cylinders too high)

So, unless then problems related to the material, with a correction of these parameters (increase of T and/or decrease of angular velocity of cylinders), it gives to possibility to the steel to follow the imposed plastic deformation, in order to decrease the defects.

Regards

Mattia DE


Il giorno lunedì 14 settembre 2015 09:38:50 UTC+2, Mehdi Vafakhah ha scritto:
Dear experts

Could you help me to identify the these defect. ( attached pictures )

or refer a guide document that provide me more information about hot rolling defects.

best regards.

 

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/64cb2c88-8d25-48d8-bed9-c68c65ff2152%40googlegroups.com.

For more options, visit https://groups.google.com/d/optout.



--
Regards,
Mr. Harish.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAE4SttF2Cz%3DpXeNRSCeLOu-HNscSLrWhEUOS8CP1mTEUNEZA%2Bg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...