Hi,

This material is highly prone to cracking when the base metal crosses certain temp.

Universally adopted method is to sink 3/4 the of base meat in a water trough & weld. While welding the base metal I.P. temp should be less than 100 deg. C.

This will definitely avoid cracking.

Check the grade of base metal & the same is available in SMAW consumables with all the manufacturers.

JS

On Jul 7, 2015 9:31 AM, "Hrushikesh Sangamnerkar" <hrushi612@gmail.com> wrote:

Main problem observed is start-stop point crack in specially SMAW. And PT is getting difficult to clear. Highly skilled welder is employed. So that possibility is ruled out of his ability and skill. Is this material prone to crack at start stop points only?

Hrushikesh H Sangamnerkar

On Jul 6, 2015 1:46 PM, "Srinivasan Jagannathan" <jsrisud@gmail.com> wrote:
Hi Hrushikesh,

What's the issue in welding Hadfield steel?

I will try to help you.

JS



On Sun, Jul 5, 2015 at 6:46 PM, Hrushikesh Sangamnerkar <hrushi612@gmail.com> wrote:

Hi..
Anyone has experience of welding Hadfield steel?

Hrushikesh H Sangamnerkar

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMpWL2q1NBcWCZkdO1jxbHMjpcWCPvcnP4%2BKuizfX3HAgDkqkw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
J.SRINIVASAN

General Manager - Technical Services.

D&H SECHERON - INDORE

Mob: 7898989756

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKHQPVxMStKRirHgUeJ2VQqwmFnOTVGgS_UKbMVak_1_gG9Wzg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMpWL2o%3Dzo9z_cQoMmY92muVcrZFRnzChcVUg3tJHPbk2yqp7A%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKHQPVzC61QWXF%2B6kqRZz9DjinbET1ZU3GFKfOW5f8di39SbZw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...