Tuesday, February 3, 2015

Re: [MW:22796] ASTM A 578 LEVEL B

Dear Ali,

8.2 refers you to the discontinuities which pass 8.1 requirements for loss in back reflection and then discuss about the size of such discontinuities.

Regards

On Mon, Feb 2, 2015 at 12:53 PM, Ali Asghari <asgharialigl@gmail.com> wrote:
Dear All
In lamination check by straight probe , some lamination and inclusion detected but they have a echo height less that 15%. Acceptance of project is level B of ASTM A578.
Now  I want to know in 8.2 of A578 , small discontinuities must have total loss of back reflection or not?
Grade of material is API 2H GR 50 Z.
Regards.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALcH7WBi%2B9cYffHt97RTS2ZnwCocUaB2oNywJP%2BVC53ZCN8Yng%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
M. Shokri Arfaei
ISA-ISTS - Metallurgy Lab. Manager
ASNT NDT Level III
International Welding Engineer

Tel.: +98 21 66282127
Fax: +98 21 66282779
Mob.:+98 912 1394023




--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAC8uMtschYQ1uzH%3DrHwfUwtQLMrE0fwtLORjktMAFLHTfbRgNw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35354] Cast-iron welding

1. Preheat joint area(other area, cover with mineral wool). 2. ENiCi or ENiFe-CI. 3. stringer bead. 4. peening is to be done on weldmetal im...