Hello,

As vanchi wrote it's important to review flux/wire class and the others essential variables

For lincoln 880-flux, and LA90-wire (EA3K), lincoln classified as F8A4
For lincoln 880M-flux, and LA90-wire, lincoln classified as F9A6

The second one has more mechanical strength, and more impact resistance,

In your are manufacturing API 5L jointers, or pipes, you will notice that API consider essential variables the following also:

1) change in the filler metal classification,
2) when impact tests are required, a change in the consumable brand name,
6) change in submerged-arc welding flux from one designation to another;

We see that API requirement is more stringent than ASME IX, to solve this problem you need to requalified with the 880 flux.

Sergio Muñoz
IWE-IIW
http://Weld-ING.tk



El domingo, 1 de febrero de 2015, 11:34:07 (UTC-5), Hamid Firoozi escribió:
Sergio
Impact is required on -4 31/22 and Wire is EA3K

Thanks

On Saturday, January 31, 2015 at 11:08:38 AM UTC-6, Sergio Antonio Muñoz Pinzón wrote:
Pelase inform what wire are you using, and what construction code, do you have impact requierements?

Sergio Muñoz
IWE-IIW
http://weld-ING.tk

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f86b3c97-e57f-4b49-896b-d8220f5c56b2%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...