Re: [MW:20943] Pipeline selection criteria

3LPE is widely used as pipeline coating in offshore pipelines. FBE has also been used successfully in salt-polluted wet soils.  Your specification shall have been specified minimum requirements for such coatings.

Best Regards

Ramin Kondori

Sr. QA/QC engineer

Yadavaran Oilfield Project

SIPC (SINOPEC)



On Fri, May 30, 2014 at 3:32 AM, Alan Denney <alan@denney1.freeserve.co.uk> wrote:

3LPE is commonly used as an external pipeline coating for offshore and onshore carbon steel pipelines. Assuming your seawater contains oxygen (it normally does) then a carbon steel pipeline will be subject to internal corrosion, and notably at the welds. The alternatives are plastic lined carbon steel, GRE or polyethylene pipe. The stainless steel alternatives which are considered to be seawater resistant are 6Mo or super-duplex (PREN greater than 40).

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sandeep Karnwal
Sent: 27 May 2014 03:43
To: materials-welding@googlegroups.com
Subject: Re: [MW:20886] Pipeline selection criteria

 

Low Mn contain coating

On 26-May-2014 11:16 AM, "Saidur Rahman" <saidur04cuet@gmail.com> wrote:

Dear Experts,

Normally  Cross-coutry pipelines are 3LPE coated (except marshy land). If i want to make a pipeline near the sea or the land contain salt water which type of coating i will choose & what will be the grade of the pipe & chemical composition?

Experts recommendations are required.

Regards,

saidur

QA/QC

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35633] IP Joint

Hello experts, I would like to know what is IP joints in piping(31.3)?  Regards Saurabh -- https://materials-welding.blogspot.com/...