Skip to main content

[MW:17939] RE: 17937] Regarding PWHT soaking, cooling rate /heating rate

Dear Shashi,

 

1.     Soaking time for P1 Material as per Table 331.1.1 ie 2.4min per mm so in your case its 46 X 2.4minutes = 110.4 minutes (minimum)

2.     Cooling rate and heating rate is not mentioned in B31.3 for P. No.1 it’s up to you while establishing the PQR,

331.1.4 Heating and Cooling does not mention anything about rates. You can refer interpretations 1-69 which clearly says no specific

Heating rates are required while performing PWHT. (see below interpretation for your ref.)

 

B31.3 Interpretations No. I 1-69

Interpretation: 1-69

 

Subject: Table 331.3.1, Requirements for Heat Treatment

Date Issued: June 9,1982

 

File: 1593

Question (I): Docs ANSI/ASME B31 .3 require specific heating rates when performing heat treatment?

Reply (1): No.

Question (2): Does the cooling rate at the bottom of Table 331.3.1 apply only to P-No. llA, Group

No.1 materials?

Reply (2): Yes.

 

Cheers

MM

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of shashi
Sent: Saturday, June 15, 2013 9:23 AM
To: materials-welding@googlegroups.com
Subject: [MW:17937] Regarding PWHT soaking, cooling rate /heating rate

 

 

Dear Expert,

                         I need to clarify regarding the heating rate/cooling rate during PWHT as per B31.3, I referred code but it is not giving clear idea or maybe I can’t interpret  properly. Please advise with code backing. If suppose I have P NO 1 material of thickness 46 mm than what would be the

1. soaking time

2. cooling rate

3. heating rate

 

regards

shashi

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...