Skip to main content

Re: [MW:18036] Reg: ASME P Numbers Clarification

ASME P-Numbers

To reduce the number of welding and brazing procedure qualifications required base metals have been assigned P-Numbers by the ASME BPVC.  Ferrous metals which have specified impact test requirements have been assigned Group Numbers within P-Numbers.

These assignments have been based on comparable base metal characteristics, such as:

  •      Composition

  •      Weldability

  •      Brazeabilit

  •      Mechanical Properties

Indiscriminant substitution of materials in a set of P-Numbers or Group Numbers may lead to problems or potentially failures.  Engineering assessment is necessary prior to a change in materials.

When a base metal with a UNS number Designation is assigned a P-Number, then a base metal listed in a different ASME material specification with the same UNS number shall be considered that P-Number.

The table below is a guide and is for instructive purposes only.  Anyone specifying materials or requirements should refer directly to the ASME Boiler and Pressure Vessel Code to specify materials, P-Numbers,  procedures, or other requirements and not rely on the table below.  The table below is only a rather incomplete and approximate summary of ASME data. 

P-Numbers

Base Metal (Typical or Example)

1

Carbon  Manganese  Steels (four Group Numbers)

2

Not Used

3

Half Molybdenum or half Chromium, half Molybdenum (three Group Numbers)

4

One and a quarter Chromium, half Molybdenum (two Group Numbers)

5A

Two and a quarter Chromium, one Molybdenum

5B

Five Chromium, half Molybdenum or nine Chromium, one Molybdenum (two Group Numbers)

5C

Chromium, Molybdenum, Vanadium (five Group Numbers)

6

Martensitic Stainless Steels (Grade 410, 415, 429) (six Group Numbers)

7

Ferritic Stainless Steels (Grade 409, 430)

8

Austenitic Stainless Steels

  •      Group 1 - Grades 304, 316, 317, 347

  •      Group 2 - Grades 309, 310

  •      Group 3 - High Manganese Grades

  •      Group 4 - High Molybdenum Grades

9A, B, C

Two to four Nickel Steels

10A, B, C, F

Various low alloy steels

10H

Duplex and Super Duplex Stainless Steel (Grades 31803, 32750)

10I

High Chromium Stainless Steel

10J

High Chromium, Molybdenum Stainless Steel

10K

High Chromium, Molybdenum, Nickel Stainless Steel

11A

Various high strength low alloy steels (six Group Numbers)

11B

Various high strength low alloy steels (ten Group Numbers)

12 to 20

Not Used

21

High Aluminum content (1000 and 3000 series)

22

Aluminum (5000 series - 5052, 5454)

23

Aluminum (6000 series – 6061, 6063)

24

Not Used

25

Aluminum (5000 series - 5083, 5086, 5456)

26 to 30

Not used

31

High Copper content

32

Brass

33

Copper Silicone

34

Copper Nickel

35

Copper Aluminum

36 to 40

Not Used

41

High Nickel content

42

Nickel, Copper - (Monel 500)

43

Nickel, Chromium, Iron - (Inconel)

44

Nickel, Molybdenum – (Hastelloy B2, C22, C276, X)

45

Nickel, Chromium

46

Nickel, Chromium, Silicone

47

Nickel, Chromium, Tungsten

47 to 50

Not Used

51, 52, 53

Titanium Alloys

61, 62

Zirconium Alloys


  
On Jun 24, 2013, at 10:12 AM, PRABU k <prabuk.engg@gmail.com> wrote:


Dear Sir,

Good Day !

Kindly Guide me whether the below mentioned ASME  P NO's   corresponds to respective Steel Types, Corrections in error if any  is most thankful.
This will help me  in selecting Proper SFA as Per ASME section II Part C.


Steel Type P NUMBER  
Carbon Steel 1
Low-Alloy Steel 3,4,5A,5B,5C,6,7,8,9A,9B,9C,11A,11B,10A,10B,10C,10F
Stainless Steel 6,7,8,10H,10I,10J,10K


Kind Regards,

PRABU K


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...